An overhead insulated power cable

By using a composite heat-resistant filler of cerium-aluminum borate whiskers and carbon black in overhead insulated cables, combined with a modifier, the problem of insufficient heat resistance of cables in high-temperature environments has been solved, significantly extending the service life of the cables.

CN118359859BActive Publication Date: 2024-11-05BEIJING TIANCHENG RUIYUAN CABLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410514803.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-11-05
Estimated Expiration
2044-04-26

AI Technical Summary

Technical Problem

Existing overhead insulated cables have insufficient heat resistance in high-temperature environments, resulting in a short service life and making it difficult to meet the needs of cable capacity expansion.

Method used

A composite heat-resistant filler was prepared by combining cerium-aluminum borate whiskers with carbon black, and then combined with low-density polyethylene. Modifying agents were added to prepare an insulating layer and a shielding layer to improve the thermal stability and electrical properties of the material.

Benefits of technology

The cable life can reach 3789-4167h at 150℃, 348-517h at 200℃, and 42-113h at 260℃, which significantly improves the heat resistance and service life of the cable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to the field of cables, in particular to an overhead insulated power cable, an overhead insulated power cable, including a core, a shielding layer and an insulating layer wrapped in sequence outside the core, and the insulating layer material includes the following raw materials by weight: 100-150 parts of low-density polyethylene, 0.5-2 parts of composite heat-resistant filler, 1-4 parts of cross-linking agent, 0.1-0.5 parts of antioxidant, and 0.1-1 parts of lubricant; the preparation method of the composite heat-resistant filler is: using borax, ammonium chloride, aluminum powder, and cerium chloride as raw materials to synthesize cerium-aluminum borate whiskers, and then using cerium-aluminum borate whiskers and carbon black to prepare composite heat-resistant fillers. The obtained cable can reach a life of 3789-4167h at an operating temperature of 150°C, a life of 348-517h at an operating temperature of 200°C, and a life of 42-113h at an operating temperature of 260°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of cables, and in particular to an overhead insulated power cable. Background Art

[0002] Overhead insulated cables have good insulation properties, electrical properties and mechanical strength. Taking into account safety, reliability, economy, easy maintenance and other factors, they are deeply loved by people and have been widely used in overhead power lines in urban power grids.

[0003] With the rapid development of the national economy, the demand for electricity in my country has been increasing continuously, which has put a heavy load on the receiving end of the urban distribution network. As the economy develops, urban construction has also developed. The land available for line corridors is getting less and less, and the pressure on corridors is increasing. It is becoming more and more difficult to build new transmission lines in cities, so that the load cannot be effectively delivered to the receiving end. In order to solve the contradiction between the growing power load and the difficulty in cable line construction, the existing technology improves the transmission capacity of the existing transmission network by tapping the potential of the existing transmission network. For example, the transmission capacity of the line is increased by increasing the transmission voltage and increasing the transmission current. Among them, without changing the transmission voltage of the existing line, increasing the allowable current carrying capacity of the conductor becomes the main direction to increase the stable transmission capacity of the system and improve the normal transmission capacity of the line. This puts higher requirements on the high compliance of the cable. It is necessary to increase the temperature tolerance and maximum operating temperature of the overhead cable to ensure the reliability of its safe operation and prevent thermal aging and electrical aging insulation failures.

[0004] In response to this, researchers added some additives to polyethylene cable insulation materials to improve the heat resistance of the insulation materials. For example, adding antioxidants can more effectively prevent the occurrence of oxidation reactions in high temperature environments, thereby improving heat resistance.

[0005] The above-mentioned prior art solutions have the following defects: after adding antioxidants, the maximum operating temperature of the insulating material can reach 90-95°C, which is increasingly unable to meet the demand for overhead cable capacity expansion, and the service life under continuous high temperature is relatively low. Summary of the invention

[0006] In order to expand the transmission capacity of the overhead insulated power cable while ensuring the service life of the cable, the present application provides an overhead insulated power cable.

[0007] The above technical objectives of this application are achieved through the following technical solutions:

[0008] An overhead insulated power cable comprises a core, a shielding layer and an insulating layer are sequentially wrapped around the core, and the insulating layer material comprises the following raw materials in parts by weight: 100-150 parts of low-density polyethylene, 0.5-2 parts of composite heat-resistant filler, 1-4 parts of cross-linking agent, 0.1-0.5 parts of antioxidant, and 0.1-1 parts of lubricant;

[0009] The preparation method of the composite heat-resistant filler is as follows:

[0010] 1) Preparation of cerium-aluminum borate whiskers

[0011] Dissolving borax and ammonium chloride respectively and mixing them, then adding aluminum powder and cerium chloride to obtain a mixed solution, heating the mixed solution to 450-550° C. and keeping the temperature constant for 9-11 hours, collecting a solid product after cooling, washing the solid product, and drying the solid product to obtain cerium-aluminum borate whiskers;

[0012] 2) Preparation of composite heat-resistant fillers

[0013] The cerium-aluminum borate whiskers obtained in step 1) are added together with carbon black into a polyvinyl alcohol solution, mixed, pressed and molded, and dried. After drying, the mixture is kept at 1000-1100° C. to obtain a composite heat-resistant filler;

[0014] The weight ratio of borax:aluminum powder:ammonium chloride is 14:1:(5-8);

[0015] The weight ratio of the cerium chloride to the aluminum powder is (5-9):100.

[0016] By adopting the above scheme, borax and aluminum powder are used as raw materials to prepare aluminum borate whiskers. Aluminum borate whiskers are inorganic whiskers with good thermal stability. Adding them to the insulating layer material can effectively improve the thermal stability of the material.

[0017] Cerium source is added to prepare cerium-aluminum borate whiskers when preparing whiskers. Cerium is a metal element with high electrical conductivity, corrosion resistance and heat resistance. Introducing cerium into whiskers can further improve the thermal stability of whiskers, and cerium has the effect of UV protection, further reducing the probability of aging of insulating materials in high temperature and outdoor exposure environments, and extending the service life of insulating materials. In addition, cerium, as a rare earth element, has a special electron layer, and it is easy to lose adjacent atoms and produce a large number of dangling bonds when combined with other elements. At this time, the rare earth element is in a high energy state, and the empty orbit needs to be filled to reduce the surface energy, thereby providing more crystal nucleus particles to inhibit the lateral growth of whiskers, resulting in whisker refinement. The refined whiskers can be more densely distributed in low-density polyethylene, which increases the contact area between the whiskers and the matrix, exerts the heat resistance of the whiskers to a greater extent, and further improves the heat resistance of the insulating material.

[0018] Ammonium chloride is added during the preparation of whiskers. The ammonium chloride decomposes to produce ammonia, which stabilizes the crystal structure and inhibits crystal transformation during the reaction, causing the whiskers to become mostly disordered. The length of the aluminum borate whiskers increases, the aspect ratio continues to expand, the whiskers are uniform in thickness, and the morphology is complete, further improving the heat resistance of the whiskers.

[0019] The cerium-aluminum borate whiskers and carbon black are compounded as composite heat-resistant fillers. Carbon black itself can be used as a heat-resistant filler to improve the heat resistance of insulating materials. During the heat treatment process of preparing the composite heat-resistant filler, the whiskers are cross-arranged around the pores left after the carbon black is burned out during the heat treatment process. Further heat treatment during the preparation of the heat-resistant material increases the diameter of the whiskers and improves the heat resistance of the whiskers.

[0020] Furthermore, the weight ratio of the low-density polyethylene to the composite heat-resistant filler is 1:(0.007-0.009).

[0021] By adopting the above technical solution, the ratio of the matrix and the heat-resistant filler is limited. The heat-resistant filler can be distributed more evenly in the matrix within the ratio range specified in this application, and the comprehensive performance of the heat resistance and mechanical properties of the prepared material is better. If the amount of heat-resistant filler added is too small, the heat resistance of the prepared material is relatively poor. If the amount of heat-resistant filler added is too large, it will agglomerate in the matrix, affecting the mechanical properties of the material.

[0022] Furthermore, the weight ratio of the cerium-aluminum borate whiskers to carbon black is 1:(3-5).

[0023] By adopting the above technical solution, the ratio of whiskers to carbon black in the composite heat-resistant filler is limited. Within the ratio range specified in the present application, the composite effect of carbon black and whiskers is better.

[0024] Furthermore, in the step of preparing the cerium-aluminum borate whiskers, sodium dodecylbenzene sulfonate is also added to the mixed solution.

[0025] By adopting the above technical solution, sodium dodecylbenzene sulfonate is added in the preparation of whiskers. Sodium dodecylbenzene sulfonate is an anionic surfactant with strong dispersing ability. It can increase the migration rate of ions in the solution and thus reduce the probability of secondary nucleation occurring during the whisker growth process, providing an excellent environment for whisker growth, obtaining whiskers with better heat resistance, and further improving the heat resistance of the insulating material.

[0026] Furthermore, the composite heat-resistant filler is modified by:

[0027] 1) Mix fluorosilicone resin, epoxy resin, curing agent, defoaming agent and diluent to obtain a resin base solution;

[0028] 2) Add the composite heat-resistant filler into the resin base solution, mix, let stand, filter, and dry to obtain a modified composite heat-resistant filler.

[0029] Furthermore, the weight ratio of the fluorosilicone resin to the epoxy resin is 1:(1-2).

[0030] By adopting the above technical solution, the heat-resistant filler is modified by compounding fluorosilicone resin and epoxy resin, which improves the bonding performance of the heat-resistant filler and the matrix on the one hand; on the other hand, the modified treatment makes the surface of the heat-resistant filler have intricate lines similar to the surface of lotus leaves. The gaps between the uneven rough structures can form an air layer, so that water droplets much larger than this structure can only form point contacts on the micro-protrusions through the air, but cannot penetrate into the gaps of the micro-protrusions, which is beneficial to improve the hydrophobicity of the material, further reduce the water absorption rate of the material, and improve the electrical properties and service life of the material. In addition, the compounding of fluorosilicone resin and epoxy resin can effectively reduce the internal stress of epoxy resin, improve the fracture strength and surface properties of epoxy resin, and enhance its toughness and heat resistance.

[0031] Furthermore, the lubricant is a fluorosilicone copolymer surfactant.

[0032] By adopting the above technical solution, the fluorosilicone copolymer is used as a lubricant to make the surface of the material smooth and hydrophobic, further reduce the water absorption rate of the material, and improve the electrical performance and service life of the material.

[0033] Furthermore, the shielding layer is a semiconductive shielding material, which includes the following raw materials in parts by weight: 20-40 parts of ethylene-octene copolymer, 100-150 parts of polypropylene, 4-6 parts of sorbitol diacetal nucleating agent, 1-2 parts of rare earth nucleating agent, 0.5-1.5 parts of nucleating aid, 1-2 parts of additive, and 35-50 parts of conductive filler.

[0034] By adopting the above technical scheme, ethylene-octene copolymer is used to modify polypropylene as a matrix, and the ethylene-octene copolymer is used to toughen and modify the polypropylene.

[0035] In the process of preparing semiconductor shielding materials, sorbitol diacetal nucleating agent and rare earth nucleating agent are added. The heterogeneous nucleation effect produced by the two nucleating agents optimizes the relaxation process and rearrangement strength of the internal chain structure of the material, refines the grains and improves the crystallization process of the material, thereby increasing the melting temperature and mechanical properties of the material, so that the material can store and release energy with the temperature change when the ambient temperature changes, effectively improving the high temperature resistance of the material. The heat-resistant shielding layer and the heat-resistant insulating layer work together to increase the service life of the cable.

[0036] In addition, using graphene nanosheets as conductive fillers, the planar structure of graphene nanosheets provides a better path for phonon conduction, which is beneficial to heat flow transmission, so that the heat generated by the core can be better transferred to the insulation layer, reducing heat accumulation in the shielding layer, which is beneficial to improving the service life of the cable.

[0037] Furthermore, the weight ratio of the sorbitol diacetal nucleating agent to the rare earth nucleating agent is (3-4):1.

[0038] By adopting the above technical solution, the ratio of the two nucleating agents is limited. Within this ratio range, the obtained material has better high temperature resistance.

[0039] Furthermore, the nucleating aid comprises hydrotalcite and dispersant in a weight ratio of 1:(3-5).

[0040] By adopting the above technical solution, the additive is an important component in the processing and application of polypropylene. The additive is conducive to the full mixing of the polypropylene base material and the nucleating agent, reducing friction, accelerating the flow rate of the fluid, improving the surface gloss of the product, and preventing the degradation and aging of the product caused by high-temperature oxidation during the processing. The additive in this ratio makes the obtained material have better high-temperature resistance.

[0041] Furthermore, the weight ratio of the olefin-octene copolymer to the polypropylene is 1:(5-7).

[0042] In summary, this application has the following technical effects:

[0043] By introducing cerium into aluminum borate whiskers and then compounding it with carbon black to prepare a composite heat-resistant filler, the heat resistance of the cable is improved. The resulting cable has a service life of 3789-4167 hours at an operating temperature of 150°C, 348-517 hours at an operating temperature of 200°C, and 42-113 hours at an operating temperature of 260°C. DETAILED DESCRIPTION

[0044] The present application is further described in detail below in conjunction with embodiments.

[0045] The raw materials in the examples of this application can be obtained from the market:

[0046] Wire core: aluminum alloy wire core, resistivity 27.1 nΩ·m;

[0047] Low-density polyethylene, brand name LDPE2047K;

[0048] The cross-linking agent is dicumyl peroxide;

[0049] The antioxidant is hindered phenol antioxidant 1010;

[0050] Lubricant: 805 fluorosilicone surfactant;

[0051] Borax, Na2B4O7·10H2O, analytical grade;

[0052] Ammonium chloride, analytical grade;

[0053] Aluminum powder, analytical grade;

[0054] Polyvinyl alcohol solution, PVA mass fraction is 5%;

[0055] Carbon black, technical grade;

[0056] Sodium dodecylbenzenesulfonate, analytical grade;

[0057] Fluorosilicone resin, DOW, LS70

[0058] Epoxy resin, epoxy resin 51, density at 25℃ is 1g / cm 3 ;

[0059] Curing agent, epoxy curing agent D230;

[0060] Defoaming agent, tributyl phosphate;

[0061] diluent, reactive diluent;

[0062] Solvent, ethyl acetate;

[0063] Ethylene-octene copolymer, melt index 2.5±0.7 g / min, 200°C, 2.16 kg;

[0064] Polypropylene, melt index 2.5 ± 0.7 g / min, 200 °C, 2.16 kg;

[0065] Sorbitol diacetal nucleating agent, NX8000K;

[0066] Rare earth nucleating agent, WBG-Ⅱ;

[0067] Dispersant, TAS-2A, purity 99.5%;

[0068] Admixture, crosslinker: antioxidant 630: pp wax in a weight ratio of 5:3:2;

[0069] Conductive filler, graphene nanosheets: size 50 μm, thickness 3-5 nm.

[0070] Preparation Example 1-6

[0071] A composite heat-resistant filler, the preparation method of which is as follows:

[0072] 1) Preparation of cerium-aluminum borate whiskers

[0073] According to the ratio in Table 1, borax and ammonium chloride were completely dissolved in water and mixed, and then aluminum powder and cerium chloride were added to obtain a mixed solution, and the mixed solution was added to a reactor, and the reactor was sealed.

[0074] Place in a muffle furnace, heat to 500°C, heating rate of 10°C / min, keep constant temperature for 10 h. After the reactor is cooled, collect the solid product, wash the solid product with concentrated hydrochloric acid, deionized water, and anhydrous ethanol, respectively, place in an oven, and dry at 120°C to obtain cerium-aluminum borate whiskers;

[0075] 2) Preparation of composite heat-resistant fillers

[0076] According to the ratio in Table 2, the cerium-aluminum borate whiskers obtained in step 1) and carbon black are added to 60L of polyvinyl alcohol solution, mixed, pressed and dried, and then kept warm at 1000°C to obtain a composite heat-resistant filler; wherein the weight ratio of cerium-aluminum borate whiskers to carbon black is 1:4.

[0077] Table 1 Ratio of raw materials of cerium-aluminum borate whiskers (kg)

[0078]

[0079] Preparation Example 10

[0080] Different from Preparation Example 2, the weight ratio of cerium-aluminum borate whiskers to carbon black in Preparation Example 10 is 1:3.

[0081] Preparation Example 11

[0082] Different from Preparation Example 2, the weight ratio of cerium-aluminum borate whiskers to carbon black in Preparation Example 11 is 1:5.

[0083] Preparation Example 12

[0084] Different from Preparation Example 2, 1 kg of sodium dodecylbenzene sulfonate was also added to the mixed solution in Preparation Example 12.

[0085] Preparation Example 13

[0086] A modified composite heat-resistant filler, the preparation method of which is as follows:

[0087] 1) Mix 10 kg of fluorosilicone resin, 10 kg of epoxy resin, 50 kg of curing agent, 0.2 kg of defoaming agent and 3 kg of diluent into 80 kg of solvent to obtain a resin base solution;

[0088] 2) 10 kg of the composite heat-resistant filler obtained in Preparation Example 11 was added to the resin base solution for mixing, allowing to stand, filtering, and drying to obtain a modified composite heat-resistant filler.

[0089] Preparation Example 14

[0090] Different from Preparation Example 13, in Preparation Example 14, 10 kg of fluorosilicone resin, 20 kg of epoxy resin, 70 kg of curing agent, 0.2 kg of defoaming agent and 3 kg of diluent were mixed and added to 100 kg of solvent to obtain a resin base solution. Example Example

[0091] An overhead insulated power cable, the preparation method of which is as follows:

[0092] S1. Wire core preparation;

[0093] S2. Wrap shielding layer:

[0094] According to the raw material ratio in Table 2, olefin-octene copolymer, polypropylene, sorbitol diacetal nucleating agent, rare earth nucleating agent, nucleating aid, additive, and conductive filler are mixed and extruded at an extrusion temperature of 100°C and wrapped around the wire core;

[0095] S3. Wrap insulation layer

[0096] According to the raw material ratio in Table 3, low-density polyethylene, composite heat-resistant filler, cross-linking agent, antioxidant and lubricant are mixed and extruded at an extrusion temperature of 120°C and wrapped outside the shielding layer.

[0097] Table 2 Raw material ratio of shielding layer materials (kg)

[0098]

[0099] Table 3 Raw material ratio of insulation layer materials (kg)

[0100]

[0101] The composite heat-resistant filler comes from Preparation Example 1, and the raw materials of the shielding layer in Examples 8-10 are the same as those in Example 2.

[0102] Examples 11-14

[0103] Different from Example 8, the composite heat-resistant fillers in Examples 11-14 come from Preparation Examples 2-5, respectively.

[0104] Examples 15-19

[0105] Different from Example 8, the composite heat-resistant fillers in Examples 15-19 come from Preparation Examples 10-14, respectively.

[0106] Comparative Example

[0107] Comparative Examples 1-4

[0108] Different from Example 1, the composite heat-resistant fillers in Comparative Examples 1-4 are from Preparation Examples 6-9.

[0109] Performance Testing

[0110] The following performance tests were performed on the cables obtained in the embodiments and comparative examples. The test results are shown in Table 4:

[0111] Service life test: The service life of the cable is tested according to the method of accelerated aging test of the sample. The maximum operating temperature of the conductor used for testing is 120℃, 150℃ and 200℃ respectively, until the insulation layer cracks;

[0112] Performance test after heat aging: Carry out high temperature test according to the method in GB / T 2951.42-2008, measure the tensile strength before and after high temperature, and record the rate of change of tensile strength.

[0113] Table 4 Performance test results

[0114]

[0115] Combining Examples 1-19 with Comparative Examples 1-4 and Table 4, it can be seen that the service life of the cable in Example 1-19 in the accelerated aging experiment is better than that of Comparative Examples 1-4, and the rate of change of the tensile strength of the cable in Example 1-19 before and after high temperature treatment is lower than that of Comparative Examples 1-4, which indicates that the high temperature resistance of the cable prepared in the present application is better.

[0116] Combining Example 1 with Comparative Examples 1-4 and Table 4, it can be seen that the heat-resistant fillers added in Comparative Examples 1-4 are different from those in Example 1, and the high temperature resistance of the cables in Comparative Examples 1-4 is significantly lower than that in Example 1, which shows that the heat-resistant fillers play an important role in the high temperature resistance of the cables. Among them, the whiskers in Comparative Examples 1 and 3 contain cerium elements, and the high temperature resistance of the cables in Comparative Examples 1 and 3 is better than that in Comparative Examples 2 and 4, which shows that the introduction of cerium elements helps to improve the high temperature resistance, which may be because, on the one hand, cerium has the effect of anti-ultraviolet rays, further reducing the probability of aging of the insulating material in high temperature and outdoor exposure environments; on the other hand, cerium, as a rare earth element, can improve the morphology of the whiskers and improve the high temperature resistance. Compared with Comparative Example 1, no ammonium chloride was added during the preparation of the whiskers in Comparative Example 3, and the high temperature resistance of the cable in Comparative Example 3 was lower than that in Comparative Example 1, which shows that adding ammonium chloride when preparing the whiskers helps to improve the high temperature resistance. This may be because ammonium chloride is added when preparing the whiskers, and the ammonium chloride decomposes to produce ammonia, which plays a role in stabilizing the crystal structure and inhibiting crystal transformation during the reaction, causing the whiskers to become mostly disordered. The length of the aluminum borate whiskers increases, the aspect ratio continues to expand, the whiskers are uniform in thickness, and the morphology is complete, which further improves the heat resistance of the whiskers.

[0117] Combining Example 11 with Example 17 and Table 4, it can be seen that, relative to Example 11, sodium dodecylbenzene sulfonate is added to the whiskers in the heat-resistant filler in the cable in Example 17 during preparation, and the high temperature resistance of the cable in Example 17 is significantly improved, which indicates that the addition of sodium dodecylbenzene sulfonate during the preparation of whiskers helps to improve the high temperature resistance. This may be because sodium dodecylbenzene sulfonate can increase the migration rate of ions in the solution, thereby reducing the probability of secondary nucleation occurring during the whisker growth process, providing an excellent environment for whisker growth, and obtaining whiskers with better heat resistance.

[0118] In combination with Examples 17-19 and Table 4, it can be seen that after the composite heat-resistant fillers in Examples 17-19 are modified, the high temperature resistance of the cables in Examples 17-19 is improved, which indicates that surface hydrophobic modification of the composite heat-resistant filling material is beneficial to improving the high temperature resistance of the cable.

[0119] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An overhead insulated power cable, characterized in that: The invention comprises a wire core, and a shielding layer and an insulating layer are wrapped around the wire core in sequence. The insulating layer material comprises the following raw materials in parts by weight: 100-150 parts of low-density polyethylene, 0.5-2 parts of composite heat-resistant filler, 1-4 parts of cross-linking agent, 0.1-0.5 parts of antioxidant, and 0.1-1 parts of lubricant; The preparation method of the composite heat-resistant filler is as follows: Preparation of Ce-Aluminum Borate Whiskers Dissolving borax and ammonium chloride in water respectively and mixing them, then adding aluminum powder and cerium chloride to obtain a mixed solution, adding the mixed solution to a reactor, sealing the reactor, heating the mixed solution to 450-550° C. for 9-11 hours, collecting a solid product after cooling, washing the solid product, and drying the solid product to obtain cerium-aluminum borate whiskers; Preparation of composite heat-resistant filler The obtained cerium-aluminum borate whiskers and carbon black are added to a polyvinyl alcohol solution, mixed, pressed into shape and dried, and then kept warm at 1000-1100° C. to obtain a composite heat-resistant filler; The weight ratio of borax:aluminum powder:ammonium chloride is 14:1:(5-8); The weight ratio of the cerium chloride to the aluminum powder is (5-9):

100.

2. An overhead insulated power cable according to claim 1, characterized in that: The weight ratio of the low-density polyethylene to the composite heat-resistant filler is 1:(0.007-0.009).

3. An overhead insulated power cable according to claim 1, characterized in that: The weight ratio of the cerium-aluminum borate whisker to the carbon black is 1:(3-5).

4. An overhead insulated power cable according to claim 1, characterized in that: In the step of preparing the cerium-aluminum borate whisker, sodium dodecylbenzene sulfonate is also added to the mixed solution.

5. An overhead insulated power cable according to claim 1, characterized in that: The composite heat-resistant filler is modified by: Mixing fluorosilicone resin, epoxy resin, curing agent, defoaming agent and diluent into a solvent to obtain a resin base solution; The composite heat-resistant filler is added into the resin base solution for mixing, standing, filtering and drying to obtain the modified composite heat-resistant filler.

6. An overhead insulated power cable according to claim 5, characterized in that: The weight ratio of the fluorosilicone resin to the epoxy resin is 1:(1-2).

7. An overhead insulated power cable according to claim 1, characterized in that: The lubricant is a fluorosilicone copolymer surfactant.

8. An overhead insulated power cable according to claim 1, characterized in that: The shielding layer is a semi-conductive shielding material, which includes the following raw materials in parts by weight: 20-40 parts of ethylene-octene copolymer, 100-150 parts of polypropylene, 4-6 parts of sorbitol diacetal nucleating agent, 1-2 parts of rare earth nucleating agent, 0.5-1.5 parts of nucleating aid, 1-2 parts of additive, and 35-50 parts of conductive filler; The additive is a cross-linking agent: antioxidant 630: pp wax in a weight ratio of 5:3:

2.

9. An overhead insulated power cable according to claim 8, characterized in that: The weight ratio of the sorbitol diacetal nucleating agent to the rare earth nucleating agent is (3-4):

1.

10. An overhead insulated power cable according to claim 8, characterized in that: The nucleating aid comprises hydrotalcite and a dispersant in a weight ratio of 1:(3-5).