A kind of DTY low-elastic network yarn and its production process
By chemically treating and polymerizing the recovered PET particles, low-elastic network wire with high fracture strength and aging resistance were prepared, which solved the problem of insufficient fracture strength and environmental pollution of the recovered PET particles in the low-elastic network wire, and achieved resources efficient utilization and environmental protection effect.
Patent Information
- Application Number
- CN202410644165.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-05-23
AI Technical Summary
When recycling PET particles is directly used to produce low-elastic network wires, their fracture strength is poor, which limits the scope of application, and there are problems of environmental pollution and resource waste.
Regenerated PET particles are used to form organic intermediate monomers through chemical substances such as itaconic anhydride, diethylenetriamine, isocyanate propyltriethoxysilane, maleic acid, etc., and under the action of crosslinking agent Perform polymerization reaction to improve the amount and compatibility of the regenerated PET particles, and combine polyamide 66 resin, polycarbonate resin, inorganic filler and other raw materials to prepare low-elastic network wires with high breaking strength and aging resistance.
It has achieved improved fracture strength of low-elastic network wire, good uniformity of strength distribution, high aging resistance, extended the stability and life of use, and reduced environmental pollution and resource waste.
Smart Images

Figure BDA0004854265380000061 
Figure BDA0004854265380000071 
Figure BDA0004854265380000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of low-elastic network yarn, and more specifically, to a DTY low-elastic network yarn and a production process thereof. Background Art
[0002] DTY low-elastic network yarn is a common textile raw material, and its raw material often uses polyester resin, polypropylene resin, spandex resin, cotton resin, etc., among which polyester resin, i.e. PET resin, has excellent wear resistance and chemical stability and is widely accepted and applied. With the extensive use of PET resin in recent years, a large amount of waste PET resin is inevitably generated. If it is directly buried, there is a hidden danger of environmental pollution and also causes a waste of resources. Some researchers propose to recycle the waste PET resin to obtain recycled PET resin, and then sort the recycled PET resin, crush, wash, dry, and obtain recycled PET particles. Further, the recycled PET particles are used for the processing and production of DTY low-elastic network yarn. However, directly using recycled PET particles to produce low-elastic network yarn has poor breaking strength, which limits the scope of application. Summary of the invention
[0003] In order to realize the application of recycled PET particles and improve the breaking strength of low-elastic network yarn, the present application provides a DTY low-elastic network yarn and a production process thereof.
[0004] In the first aspect, the present application provides a DTY low-elastic network yarn, which adopts the following technical solution:
[0005] A low-elastic network yarn is mainly made of the following raw materials in parts by weight: 50-70 parts of recycled PET particles, 15-25 parts of polyamide 66 resin, 15-25 parts of polycarbonate resin, 1-3 parts of coupling agent, 5-10 parts of inorganic filler, and 5-10 parts of antioxidant; the recycled PET particles are obtained by treating recycled PET particles with itaconic anhydride, diethylenetriamine, isocyanate propyltriethoxysilane, and maleic acid.
[0006] By adopting the above technical scheme, the low-elastic network yarn of the present application not only realizes the application of recycled PET particles, reduces environmental pollution, and reduces resource waste. In addition, by processing the recycled PET particles to obtain regenerated PET particles, and utilizing the synergistic enhancement between itaconic anhydride, diethylenetriamine, isocyanatepropyltriethoxysilane, and maleic acid, the low-elastic network yarn has a pre-aging breaking strength of >3cN / dtex, a pre-aging breaking strength CV value of <4%, and an aging breaking strength loss rate of <9%, showing the advantages of high breaking strength, good uniformity of strength distribution, and high aging resistance, increasing the use stability and life of the low-elastic network yarn and meeting market demand.
[0007] Optionally, the recycled PET particles are prepared by the following method:
[0008] T1, mixing toluene and diethylenetriamine to obtain a premixed solution;
[0009] T2, mixing toluene and itaconic anhydride, adding the premixed liquid dropwise, and distilling under reduced pressure to obtain an organic intermediate monomer;
[0010] T3, soaking the recovered PET particles in a sulfuric acid aqueous solution, taking them out, drying them, and irradiating them with ultraviolet light to obtain activated PET particles;
[0011] T4, mixing activated PET particles, isocyanate propyl triethoxysilane, maleic acid, organic intermediate monomer, and crosslinking agent, melt-extruding, cooling and granulating, and obtaining recycled PET particles.
[0012] Optionally, the weight ratio of the activated PET particles, isocyanatepropyltriethoxysilane, maleic acid, organic intermediate monomer, and cross-linking agent is 100:(4-6):(9-11):(4-6):(0.1-0.5).
[0013] By adopting the above technical scheme, the anhydride group in itaconic anhydride and the secondary amine group in diethylenetriamine are reacted in advance to form an organic intermediate monomer, which contains a carbon-carbon double bond, a carboxyl group and a primary amine group.
[0014] Soaking the recycled PET particles in a sulfuric acid aqueous solution can effectively increase the amount of hydroxyl and carboxyl groups on the surface of the recycled PET particles. Combined with ultraviolet irradiation treatment, the amount of active groups can be further increased to achieve the activation of the recycled PET particles. After that, the activated PET particles, triethoxypropyl isocyanate silane, maleic acid, an organic intermediate monomer, and a crosslinking agent are mixed. The isocyanate group in triethoxypropyl isocyanate silane can react with the hydroxyl groups on the surface of the activated PET particles, and the carboxyl groups in maleic acid and the carboxyl groups in the organic intermediate monomer can react with the hydroxyl groups on the surface of the activated PET particles. At the same time, a polymerization reaction can also occur under the action of the crosslinking agent, and a large number of active groups such as siloxy, carboxyl, and primary amine groups are introduced on the surface, thereby improving the compatibility, bonding force, crosslinking density, and integrity of the recycled PET particles and polyamide 66 resin, polycarbonate resin, and inorganic filler, so that the low-elastic network yarn exhibits better breaking strength and aging resistance.
[0015] Optionally, the weight ratio of itaconic anhydride and diethylenetriamine in the premix is (8-12):(5-7).
[0016] By adopting the above technical solution, the weight ratio of itaconic anhydride and diethylenetriamine in the premix is optimized to make itaconic anhydride excessive, ensure the reaction between the anhydride group in itaconic anhydride and the secondary amine group in diethylenetriamine, and reduce side reactions. In multiple implementation schemes, the weight ratio of itaconic anhydride and diethylenetriamine in the premix is 5:3, and the weight ratio can also be set to 8:5, 4:3, 8:7, 2:1, 10:7, 12:5, 12:7 as needed, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0017] Further, in step S1, the weight ratio of toluene and diethylenetriamine in the premix is (5-15): 1. In multiple embodiments, the weight ratio of toluene and diethylenetriamine in the premix is 10: 1, and the weight ratio can also be set to 5: 1, 6: 1, 7: 1, 8: 1, 9: 1, 11: 1, 12: 1, 13: 1, 14: 1, 15: 1 as needed, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] Further, in step S2, the addition time of the premix is 20-60min, and the stirring process is continued for 30-120min after the dropwise addition is completed. In multiple embodiments, the addition time of the premix is 30min, and the addition time can also be set to 20min, 40min, 50min, 60min as needed, but is not limited to the listed numerical values, and other unlisted numerical values in the numerical range are equally applicable. In multiple embodiments, the addition is continued for 60min after the dropwise addition is completed, and the addition time can also be set to 30min, 40min, 50min, 70min, 80min, 90min, 100min, 110min, 120min as needed, but is not limited to the listed numerical values, and other unlisted numerical values in the numerical range are equally applicable.
[0019] Further, in step T3, the weight ratio of the recovered PET particles and the aqueous sulfuric acid solution is 1: (1-5), the mass concentration of sulfuric acid in the aqueous sulfuric acid solution is 5-20%, and the soaking treatment time is 10-120 min. In multiple embodiments, the weight ratio of the recovered PET particles and the aqueous sulfuric acid solution is 1: 2, and the weight ratio can also be set to 1: 1, 1: 3, 1: 4, 1: 5 as needed, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable. In multiple embodiments, the mass concentration of sulfuric acid in the aqueous sulfuric acid solution is 10%, and the mass concentration can also be set to 5%, 8%, 13%, 15%, 18%, 20% as needed, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable. In multiple embodiments, the immersion treatment time is 30 minutes, and the time can also be set to 10 minutes, 20 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, 100 minutes, 110 minutes, 120 minutes as needed, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] In step T3, the power of ultraviolet irradiation is 0.5-3KW and the time is 10-30min. In multiple embodiments, the power of ultraviolet irradiation is 1KW, and the power can also be set to 0.5KW, 1.5KW, 2KW, 2.5KW, 3KW as needed, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable. In multiple embodiments, the time of ultraviolet irradiation is 15min, and the time can also be set to 10min, 13min, 18min, 20min, 23min, 25min, 28min, 30min as needed, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0021] Optionally, the cross-linking agent is one or more of benzoyl peroxide, methyl ethyl ketone peroxide, tert-butyl perbenzoate, and azobisisobutyronitrile.
[0022] By adopting the above technical solution, the crosslinking agent is optimized, which facilitates the selection of the crosslinking agent. Moreover, benzoyl peroxide, methyl ethyl ketone peroxide, tert-butyl perbenzoate, and azobisisobutyronitrile can release free radicals and promote the polymerization reaction of organic monomers, increase the grafting stability, and ensure the stability of the preparation of recycled PET particles.
[0023] Further, in step S4, the melting temperature is 270-300° C. In many embodiments, the melting temperature is 290° C., and the melting temperature can also be set to 270° C., 280° C., 300° C. as required, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0024] Optionally, the recycled PET particles are prepared by the following method: recycled PET slices are sorted, crushed, washed, and dried to obtain pretreated recycled PET particles.
[0025] By adopting the above technical solution, the recycled PET chips are crushed to facilitate the mixing of raw materials. The recycled PET chips are also sorted and washed to reduce impurities, thereby ensuring the quality of the recycled PET particles and thus ensuring the stability of the production of low-elastic network yarns.
[0026] Further, the intrinsic viscosity of the recycled PET chips is 0.5-0.8 dl / g, and the intrinsic viscosity of the recycled PET chips is measured by the method of ASTM D4603. In multiple embodiments, the intrinsic viscosity of the recycled PET chips is 0.65 dl / g, and the intrinsic viscosity can also be set to 0.5 dl / g, 0.6 dl / g, 0.7 dl / g, 0.8 dl / g as needed, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0027] Furthermore, the average particle size of the recycled PET particles is 0.1-5 mm. In multiple embodiments, the average particle size of the recycled PET particles is 0.5 mm, and the average particle size can also be set to 0.1 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm as needed, but is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0028] Optionally, the inorganic filler is one or more of titanium dioxide, silicon dioxide, graphene, graphene oxide, microsilica powder, talcum powder, and mica powder.
[0029] By adopting the above technical solution, the inorganic filler is optimized, which facilitates the selection of the inorganic filler. Further, the inorganic filler is titanium dioxide, and the average particle size of titanium dioxide is 1-10 μm. Preferably, the average particle size of titanium dioxide is 1-5 μm. In multiple embodiments, the average particle size of titanium dioxide is 2 μm, and the average particle size can also be set to 1 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm as needed, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Optionally, the antioxidant is one or more of antioxidant 1010, antioxidant 626, antioxidant 1076, antioxidant 2246, and antioxidant 168;
[0031] The coupling agent is one or more of silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570, silane coupling agent A151, and silane coupling agent DL602.
[0032] By adopting the above technical solution, antioxidants and coupling agents are optimized, which facilitates the selection of antioxidants and coupling agents. Further, the antioxidants are two kinds of antioxidants, antioxidant 1010 and antioxidant 168, and the weight ratio of antioxidant 1010 and antioxidant 168 is (1-3): (1-3). In multiple embodiments, the weight ratio of antioxidant 1010 and antioxidant 168 is 2:1, and the weight ratio can also be set to 1:1, 1:2, 1:3, 2:3, 3:1, 3:2 as needed, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] Furthermore, the polyamide 66 resin is polyamide 66 resin EP-158, and the polycarbonate resin is polycarbonate resin L-1225Z100K.
[0034] In a second aspect, the present application provides a production process of the DTY low-elastic network yarn, which adopts the following technical solution:
[0035] A production process of the DTY low-elastic network yarn comprises the following steps:
[0036] S1. Mixing: Mixing recycled PET particles, polyamide 66 resin, polycarbonate resin, coupling agent, inorganic filler, and antioxidant to obtain a mixture;
[0037] S2, POY process: the mixed material is metered, melt-extruded, spun, cooled, oiled, and wound to obtain POY polyester filament;
[0038] S3, DTY process: POY polyester filament is guided, heated and stretched, cooled, false twisted, netted, heat-set, and wound to obtain DTY polyester stretch yarn;
[0039] S4. Heat treatment: heat-treat the DTY polyester stretch yarn to obtain a low-elastic network yarn.
[0040] By adopting the above technical solution, the preparation of low-elastic network yarn is facilitated, and the obtained DTY polyester elastic yarn is subjected to heat treatment to increase the stability of the DTY polyester elastic yarn and ensure the quality of the low-elastic network yarn.
[0041] Optionally, in step S2, the spinning temperature is 280-290°C;
[0042] In step S3, the temperature of heating and stretching is 170-190°C, the stretching ratio is 1.15-1.25; the D / Y ratio of false twist is 1.65-1.75; the pressure of netting is 1.3-1.6 bar; the temperature of heat setting is 160-180°C;
[0043] In step S4, the heat treatment temperature is 120-140° C. and the time is 1-2 h.
[0044] By adopting the above technical solution, the temperature of the spinning is limited, which is convenient for the melting of the mixed material and the formation of filaments. The temperature of the heating and stretching, the stretching multiple, the D / Y ratio of the false twist, the netting pressure and the heat setting stability are also limited, which is convenient for the preparation of DTY polyester stretch yarn. The temperature and time of the heat treatment are also limited to ensure the stability and quality of the production of low-elastic network yarn.
[0045] In summary, this application has the following beneficial effects:
[0046] 1. The low-elastic network yarn of the present application has a breaking strength before aging of >3cN / dtex, a breaking strength CV value before aging of <4%, and a breaking strength loss rate after aging of <9%, showing the advantages of high breaking strength, good uniformity of strength distribution, and high aging resistance, meeting market demand.
[0047] 2. In the method for preparing recycled PET particles, an organic intermediate monomer is prepared in advance, and then the recycled PET particles are soaked in acid solution and irradiated with ultraviolet light to increase the amount of surface active groups. Thereafter, isocyanatepropyltriethoxysilane, maleic acid, and an organic intermediate monomer are grafted, and the organic monomer is polymerized with the help of a cross-linking agent to introduce a large number of active groups such as siloxy, carboxyl, and primary amine groups on the surface, thereby improving the compatibility, bonding strength, cross-linking density, and integrity between the recycled PET particles and the raw materials, so that the low-elastic network yarn exhibits better breaking strength and aging resistance. DETAILED DESCRIPTION
[0048] In order to make the present application easier to understand, the present application will be further described in detail below in conjunction with the examples, which are merely illustrative and are not intended to limit the scope of application of the present application. The raw materials or components used in the present application can be obtained through commercial routes or conventional methods unless otherwise specified.
[0049] Preparation Example
[0050] Preparation Example 1
[0051] A recycled PET particle is prepared by the following method:
[0052] T0. Sorting, crushing, washing and drying 200 g of recycled PET slices to obtain pretreated recycled PET particles.
[0053] The intrinsic viscosity of the recycled PET chips is 0.65 dl / g, and the intrinsic viscosity of the recycled PET chips is measured using the ASTM D4603 method; the average particle size of the recycled PET particles is 0.5 mm.
[0054] T1. Add 6 g of diethylenetriamine to 60 g of toluene and stir for 3 min to obtain a premixed solution.
[0055] T2, add 10 g of itaconic anhydride to 100 g of toluene, and stir for 3 min. Then add 66 g of the premix obtained in step S1 dropwise for 30 min, and stir for 60 min after the addition is complete. Then, perform vacuum distillation to remove toluene and remaining itaconic anhydride to obtain an organic intermediate monomer.
[0056] T3, 150g of the pre-treated recycled PET particles obtained in step S0 were soaked in 300g of a 10% sulfuric acid aqueous solution for 30 minutes, taken out, dried, and then irradiated for 15 minutes at a power of 1KW ultraviolet to obtain activated PET particles.
[0057] T4, add 5g of isocyanatepropyl triethoxysilane, 10g of maleic acid, 5g of organic intermediate monomer, and 0.2g of cross-linking agent-benzoyl peroxide to 100g of the activated PET particles obtained in step S3, stir for 3min, then melt extrude at a melting temperature of 290°C, cool and granulate to obtain recycled PET particles.
[0058] Preparation Example 2
[0059] A kind of recycled PET particles, which differ from Preparation Example 1 in that, in step T4, the added amounts of isocyanate propyl triethoxy silane, maleic acid, organic intermediate monomer, and cross-linking agent are different, and the added amount of isocyanate propyl triethoxy silane is 4g, the added amount of maleic acid is 11g, the added amount of organic intermediate monomer is 6g, and the added amount of cross-linking agent is 0.1g.
[0060] Preparation Example 3
[0061] A kind of recycled PET particles, which differ from Preparation Example 1 in that, in step T4, the added amounts of isocyanate propyl triethoxy silane, maleic acid, organic intermediate monomer, and cross-linking agent are different, and the added amount of isocyanate propyl triethoxy silane is 6g, the added amount of maleic acid is 9g, the added amount of organic intermediate monomer is 4g, and the added amount of cross-linking agent is 0.5g.
[0062] Example
[0063] Table 1 Amount of each raw material used in low-elastic network yarn (unit: × 100g)
[0064]
[0065]
[0066] Example 1
[0067] A DTY low-elastic network yarn, the raw materials and raw material ratios of which are shown in Table 1.
[0068] Among them, the polyamide 66 resin is polyamide 66 resin EP-158, and is selected from Zhejiang Huafeng; the polycarbonate resin is polycarbonate resin L-1225Z100K, and is selected from Teijin; the coupling agent is silane coupling agent KH550; the inorganic filler is titanium dioxide, and the average particle size of titanium dioxide is 2μm; the antioxidants are antioxidant 1010 and antioxidant 168, and the weight ratio of antioxidant 1010 to antioxidant 168 is 2:1; the recycled PET particles are prepared by the method of Preparation Example 1.
[0069] A production process of DTY low-elastic network yarn comprises the following steps:
[0070] S1. Mixing: Add polyamide 66 resin, polycarbonate resin, coupling agent, inorganic filler and antioxidant to recycled PET particles, stir for 3 minutes, and obtain a mixture.
[0071] S2. POY process: The mixed material is measured, melt-extruded, spun at a temperature of 290°C, cooled, oiled, and wound to obtain POY polyester filament.
[0072] S3, DTY process: The POY polyester filament is guided through the yarn, heated and stretched at a temperature of 180°C and a stretching multiple of 1.2, cooled, false-twisted at a D / Y ratio of 1.7 in a false twister, netted at a pressure of 1.6 bar in a netting machine, heat-set at a temperature of 170°C, and wound to obtain DTY polyester stretch yarn.
[0073] S4. Heat treatment: heat-treat the DTY polyester stretch yarn at 130°C for 1.5h, cool it to 23°C, and obtain a low-elastic network yarn.
[0074] Example 2
[0075] A DTY low-elastic network yarn, which is different from Example 1 in that the raw material ratio of the low-elastic network yarn is different, and the raw material ratio is shown in Table 1.
[0076] Example 3
[0077] A DTY low-elastic network yarn, which is different from Example 1 in that the raw material ratio of the low-elastic network yarn is different, and the raw material ratio is shown in Table 1.
[0078] Example 4
[0079] A DTY low-elastic network yarn, which is different from Example 1 in that the raw material ratio of the low-elastic network yarn is different, and the raw material ratio is shown in Table 1.
[0080] Example 5
[0081] A DTY low-elastic network yarn, which is different from Example 1 in that the raw material ratio of the low-elastic network yarn is different, and the raw material ratio is shown in Table 1.
[0082] Example 6
[0083] A DTY low-elastic network yarn, which is different from Example 2 in that the source of the recycled PET particles is different, and the recycled PET particles are prepared by the method of Preparation Example 2.
[0084] Example 7
[0085] A DTY low-elastic network yarn, which is different from Example 2 in that the source of the recycled PET particles is different, and the recycled PET particles are prepared by the method of Preparation Example 3.
[0086] Comparative Example
[0087] Comparative Example 1
[0088] A DTY low-elastic network yarn, which is different from Example 2 in that an equal amount of recycled PET particles are used to replace the regenerated PET particles in the raw materials of the low-elastic network yarn.
[0089] The recycled PET particles are prepared by the following method: 200 g of recycled PET slices are sorted, crushed, washed, and dried to obtain recycled PET particles.
[0090] The intrinsic viscosity of the recycled PET chips is 0.65 dl / g, and the intrinsic viscosity of the recycled PET chips is measured using the ASTM D4603 method; the average particle size of the recycled PET particles is 0.5 mm.
[0091] Comparative Example 2
[0092] A DTY low-elastic network yarn, which differs from Example 2 in that, in the preparation method of recycled PET particles in the low-elastic network yarn raw material, an equal amount of isocyanatepropyltriethoxysilane is used to replace maleic acid and organic intermediate monomers.
[0093] Comparative Example 3
[0094] A DTY low-elastic network yarn, which differs from Example 2 in that, in the preparation method of recycled PET particles in the low-elastic network yarn raw material, isocyanatepropyltriethoxysilane and organic intermediate monomer are replaced by equal amounts of maleic acid.
[0095] Comparative Example 4
[0096] A DTY low-elastic network yarn, which differs from Example 2 in that in the preparation method of recycled PET particles in the low-elastic network yarn raw material, isocyanatepropyltriethoxysilane and maleic acid are replaced by an equal amount of organic intermediate monomers.
[0097] Performance Testing
[0098] (1) The low-elastic network yarns obtained in Examples 1-7 and Comparative Examples 1-4 were respectively taken and tested according to BB / T0060-2012. After testing, the low-elastic network yarns obtained in Examples 1-7 and Comparative Examples 1-4 met the requirements of GB13113-1991.
[0099] (2) The low-elastic network yarns obtained in Examples 1-7 and Comparative Examples 1-4 were respectively taken as samples, and the following performance tests were performed on the samples. The test results are shown in Table 2.
[0100] Among them, according to GB / T14344-2008 "Test method for tensile properties of chemical fiber filaments", the breaking strength and breaking strength CV value of the sample were tested, and the smaller the breaking strength CV value, the more uniform the breaking strength distribution of the low-elastic network yarn and the more stable the quality.
[0101] The aging resistance is tested by the following method: the sample is placed at a temperature of 85°C and a humidity of 80% for 1000 hours to obtain an aged sample. The fracture strength of the aged sample is then tested and the aging fracture strength loss rate is calculated.
[0102] Furthermore, aging breaking strength loss rate / (%)=(breaking strength before aging-breaking strength after aging) / breaking strength before aging×100%.
[0103] Table 2 Test results
[0104]
[0105] As can be seen from Table 2, the low-elastic network yarn of the present application has a breaking strength of 3.37-3.76 cN / dtex before aging and a CV value of breaking strength of 3.34-3.67% before aging, showing higher breaking strength and uniformity of strength distribution. Moreover, the breaking strength after aging is 3.10-3.47 cN / dtex and the aging breaking strength loss rate is 7.71-8.19%, showing higher aging resistance and extending the stability and life of use.
[0106] Comparing Example 2 with Comparative Example 1, recycled PET particles are added to the raw material of the low-elastic network yarn in Comparative Example 1, and recycled PET particles are added to the raw material of the low-elastic network yarn in Example 2. It can be seen that grafting and modifying the recycled PET particles can improve the performance of the recycled PET particles and make the low-elastic network yarn show better breaking strength and aging resistance.
[0107] Comparing Example 2 with Comparative Examples 2-4, the recycled PET particles in the low-elastic network yarn raw material of Comparative Example 2 are treated with isocyanate propyl triethoxysilane to recover the PET particles; the recycled PET particles in the low-elastic network yarn raw material of Comparative Example 3 are treated with maleic acid to recover the PET particles; the recycled PET particles in the low-elastic network yarn raw material of Comparative Example 4 are treated with an organic intermediate monomer to recover the PET particles; the recycled PET particles in the low-elastic network yarn raw material of Example 2 are treated with isocyanate propyl triethoxysilane, maleic acid, and an organic intermediate monomer to recover the PET particles. It can be seen that the recycled PET particles are treated with isocyanate propyl triethoxysilane, maleic acid, and an organic intermediate monomer to achieve grafting and increase the grafting stability, and active groups such as siloxy, carboxyl, and primary amine groups are introduced on the surface of the recycled PET particles to improve the compatibility, bonding force, and integrity between the raw materials, enhance the fracture strength and aging resistance of the low-elastic network yarn, and make the low-elastic network yarn show better comprehensive performance.
[0108] It should be noted that the embodiments described above are only used to explain the present application and do not constitute any limitation to the present application. The present application is described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present application may be modified as specified within the scope of the claims of the present application, and the present invention may be revised without departing from the scope and spirit of the present application. Although the present application described therein relates to specific methods, materials and embodiments, it does not mean that the present application is limited to the specific examples disclosed therein. On the contrary, the present application can be extended to all other methods and applications with the same functions.
Claims
1. A DTY low-elastic network yarn, characterized by: The low-elastic network yarn is mainly made of the following raw materials in parts by weight: 50-70 parts of recycled PET particles, 15-25 parts of polyamide 66 resin, 15-25 parts of polycarbonate resin, 1-3 parts of coupling agent, 5-10 parts of inorganic filler, and 5-10 parts of antioxidant; the recycled PET particles are obtained by treating recycled PET particles with itaconic anhydride, diethylenetriamine, isocyanate propyltriethoxysilane, and maleic acid; The recycled PET particles are prepared by the following method: T1, mixing toluene and diethylenetriamine to obtain a premixed solution; T2, mixing toluene and itaconic anhydride, adding the premixed liquid dropwise, and distilling under reduced pressure to obtain an organic intermediate monomer; T3, soaking the recovered PET particles in a sulfuric acid aqueous solution, taking them out, drying them, and irradiating them with ultraviolet light to obtain activated PET particles; T4, mixing activated PET particles, isocyanate propyl triethoxysilane, maleic acid, an organic intermediate monomer, and a cross-linking agent, melt-extruding, cooling and granulating, and obtaining recycled PET particles; The weight ratio of the activated PET particles, isocyanate propyl triethoxysilane, maleic acid, organic intermediate monomer, and crosslinking agent is 100:(4-6):(9-11):(4-6):(0.1-0.5); The weight ratio of itaconic anhydride and diethylenetriamine in the premix is (8-12):(5-7); The cross-linking agent is one or more of benzoyl peroxide, methyl ethyl ketone peroxide, tert-butyl perbenzoate, and azobisisobutyronitrile.
2. The DTY low-elastic network yarn according to claim 1, characterized in that: The recycled PET particles are prepared by the following method: recycled PET slices are sorted, crushed, washed, and dried to obtain pre-treated recycled PET particles.
3. The DTY low-elastic network yarn according to claim 1, characterized in that: The inorganic filler is one or more of titanium dioxide, silicon dioxide, graphene, graphene oxide, microsilica powder, talcum powder, and mica powder.
4. The DTY low-elastic network yarn according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1010, antioxidant 626, antioxidant 1076, antioxidant 2246, and antioxidant 168; The coupling agent is one or more of silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570, silane coupling agent A151, and silane coupling agent DL602.
5. A production process of the DTY low-elastic network yarn according to any one of claims 1 to 4, characterized in that: The steps include: S1. Mixing: mixing recycled PET particles, polyamide 66 resin, polycarbonate resin, coupling agent, inorganic filler, and antioxidant to obtain a mixture; S2, POY process: the mixed material is metered, melt-extruded, spun, cooled, oiled, and wound to obtain POY polyester filament; S3, DTY process: POY polyester filament is guided, heated and stretched, cooled, false twisted, netted, heat-set, and wound to obtain DTY polyester stretch yarn; S4. Heat treatment: heat-treat the DTY polyester stretch yarn to obtain a low-elastic network yarn.
6. The production process of DTY low-elastic network yarn according to claim 5, characterized in that: In step S2, the spinning temperature is 280-290°C; In step S3, the temperature of heating and stretching is 170-190°C, the stretching ratio is 1.15-1.25; the D / Y ratio of false twist is 1.65-1.75; the pressure of netting is 1.3-1.6 bar; the temperature of heat setting is 160-180°C; In step S4, the heat treatment temperature is 120-140° C. and the time is 1-2 h.