A safety test method for titanium alloy high-pressure gas cylinders

Through low-temperature fracture toughness and cylinder fatigue test methods, the problem of safety evaluation of titanium alloy high-pressure gas cylinders in low-temperature environments has been solved, accurate safety performance evaluation has been provided, and the safety of titanium alloy high-pressure gas cylinders in marine environments has been ensured. Reduced risks in submarine use.

CN118362429BActive Publication Date: 2024-10-01CHINA STATE SHIPBUILDING CORP LTD RESEARCH INSTITUTE 719
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410783144.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

The existing technology lacks an effective safety test method for titanium alloy high-pressure gas cylinders in low-temperature environments. As a result, the low-temperature brittleness of materials when used in marine environments has not been accurately evaluated, which may cause the failure fatigue life of high-pressure gas cylinders to be significantly higher than the actual value, affecting Submarine safety.

Method used

The low-temperature fracture toughness test and gas cylinder fatigue test methods are adopted, including prefabricating fatigue cracks on titanium alloy high-pressure gas cylinder specimens, and applying load in a low-temperature environment. The hydraulic cycle fatigue test is conducted through a hydraulic cycle fatigue test device to judge the titanium alloy. Safety of high-pressure gas cylinders.

Benefits of technology

It provides an evaluation of the extreme safety performance of titanium alloy high-pressure gas cylinders in low-temperature environments, verifies the "leak but not explode" failure mode, ensures the safety of gas cylinder selection, and reduces safety risks in submarine use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118362429B_ABST
    Figure CN118362429B_ABST
Patent Text Reader

Abstract

The present invention discloses a safety test method for titanium alloy high-pressure gas cylinders, which conducts a low-temperature fracture toughness test on a sample and a cylinder fatigue test on a titanium alloy high-pressure gas cylinder prototype; provides a basis for the safety analysis of the use of titanium alloy high-pressure gas cylinders under low-temperature conditions based on the low-temperature fracture toughness, and analyzes the safety of titanium alloy high-pressure gas cylinders by whether the high-pressure gas cylinder prototype explodes and whether there is obvious deformation. The present invention can more accurately evaluate the ultimate safety performance of titanium alloy high-pressure gas cylinders in low-temperature environments, provide basic data for titanium alloy high-pressure gas cylinder material fracture analysis and gas cylinder failure analysis, verify the failure mode of "only leaking but not exploding" of high-pressure gas cylinders, and ensure the safety of actual use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium alloy high-pressure gas cylinders, and in particular to a safety testing method for titanium alloy high-pressure gas cylinders. Background Art

[0002] There are many high-pressure gas cylinders in submarines, which store high-pressure air and are necessary equipment for submarines to surface. In the past, high-pressure gas cylinders were made of steel, but titanium and titanium alloys are increasingly valued in marine engineering due to their light weight, high specific strength and superior corrosion resistance. Among them, the use of titanium alloy to make high-pressure gas cylinders is one of the applications in marine engineering. In order to ensure that high-pressure gas cylinders made of titanium alloy can meet the use requirements in marine environments, the safety of the use of gas cylinders will be verified before selecting titanium alloy high-pressure gas cylinders to avoid problems during use. However, in the marine environment, the lowest ambient temperature outside the pressure-resistant hull is as low as tens of degrees below zero, and the difference between the lowest ambient temperature and the highest ambient temperature is close to 100°C. In particular, when a high-pressure gas cylinder leaks, the material temperature of the gas cylinder will be lower. The low-temperature environment will cause the titanium alloy material to become brittle at low temperatures. The existing technology lacks an effective test method for the safety of titanium alloy high-pressure gas cylinders in low-temperature environments. At present, the prediction of the failure fatigue life of high-pressure gas cylinders in the existing technology is significantly higher than the actual failure fatigue life during use. Therefore, it is urgent to propose a method that can accurately test the safety performance of titanium alloy high-pressure gas cylinders to ensure the safety of titanium alloy high-pressure gas cylinders during actual use and to ensure the safety of submarines. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a safety testing method for a titanium alloy high-pressure gas cylinder.

[0004] The present application embodiment provides a titanium alloy high-pressure gas cylinder safety testing method, comprising:

[0005] Preparing a titanium alloy high-pressure gas cylinder test piece to be tested, wherein the test piece comprises a three-point bending specimen cut from a titanium alloy high-pressure gas cylinder pipe and a titanium alloy high-pressure gas cylinder prototype;

[0006] Performing a low-temperature fracture toughness test on the sample, wherein the low-temperature fracture toughness test includes prefabricating a fatigue crack on the sample, placing the sample in a preset low-temperature environment, applying a load to the sample, and calculating the low-temperature fracture toughness after the sample is fractured;

[0007] A cylinder fatigue test is performed on the titanium alloy high-pressure gas cylinder prototype, wherein the cylinder fatigue test includes prefabricating the cylinder prototype with cracks, arranging a plurality of strain gauges around the prefabricated cracks, performing strain testing through pressure increase and decrease cycles, and performing a hydraulic cycle fatigue test through a hydraulic fatigue test device;

[0008] The safety of the titanium alloy high-pressure gas cylinder is judged based on the low-temperature fracture toughness, whether the high-pressure gas cylinder prototype explodes, and whether there is obvious deformation.

[0009] In one embodiment, the three-point bending specimens are cut into longitudinal and transverse three-point bending specimens respectively according to a preset ratio of width to thickness.

[0010] In one embodiment, placing the sample in a preset low-temperature environment includes: injecting a liquid cooling medium into a low-temperature tank, and continuously adding liquid nitrogen to the liquid cooling medium for stirring; continuously detecting the liquid cooling medium in the low-temperature tank using a temperature detection component until the temperature reaches a preset test temperature, then stopping adding liquid nitrogen and keeping the temperature, and placing the three-point bending tester in the low-temperature tank.

[0011] In one embodiment, prefabricating fatigue cracks on the sample includes:

[0012] forming a notch in the specimen;

[0013] The fatigue loading method is used to generate a crack of preset length at the top of the notch.

[0014] The preset ratio of width to thickness and the length of the preset crack should satisfy the following relationship:

[0015]

[0016]

[0017] Where: - initial thickness of the specimen, - initial width of the specimen, L - length of the intended crack, - Width of specimen.

[0018] In one embodiment, applying a load to the sample includes: providing a lower support member in the low temperature tank, placing the sample in the low temperature tank and supporting the middle part of the lower surface of the sample by the lower support member, and applying an upward load to the lower support member by a testing machine;

[0019] An extensometer is arranged at the notch position of the specimen to output the relative displacement of the two sides of the notch at a precise location;

[0020] A first loading member and a second loading member are respectively arranged on both sides of the extensometer, and the first loading member and the second loading member are used to apply an equal vertical downward force to the upper surface of the sample.

[0021] In one embodiment, the height of the lower support member is less than the depth of the low temperature tank, and the rate of applying the load to the sample is 1 mm / min.

[0022] In one embodiment, the prefabrication crack treatment of the gas cylinder prototype includes prefabrication of axial cracks on the outer surface of the middle portion of the prototype bottle body.

[0023] In one embodiment, the arrangement of multiple strain gauges around the prefabricated crack and the strain test through pressure increase and decrease cycles include: arranging three-dimensional strain gauges at four measuring points around the prefabricated crack, and arranging two-dimensional strain gauges at two measuring points on the surface of the gas cylinder away from the prefabricated crack; the strain test includes two training cycles and one measurement cycle, and the maximum pressure of the measurement cycle is greater than the maximum pressure of the training cycle.

[0024] In one embodiment, the hydraulic cyclic fatigue test performed by the hydraulic fatigue testing device includes: applying a trapezoidal wave load to the prototype, with a test frequency of <5 times / minute, stopping after every 50 fatigue cycles, using acoustic waves to detect the size, depth and direction of prefabricated cracks, and continuing the fatigue test until the set fatigue number is reached or the gas cylinder fails.

[0025] In one embodiment, the pressure value of the hydraulic cycle fatigue test is between 3 MPa and 50 MPa.

[0026] Compared with the prior art, the above technical solution provided by the embodiment of the present application has the following beneficial effects:

[0027] A test method is proposed for conducting low-temperature fracture toughness tests and cylinder fatigue tests on specimens and prototypes of titanium alloy high-pressure gas cylinders. This method can more accurately evaluate the ultimate safety performance of titanium alloy high-pressure gas cylinders in low-temperature environments, provide basic data for material fracture analysis and cylinder failure analysis of titanium alloy high-pressure gas cylinders, verify the failure mode of "only leakage but not explosion" of high-pressure gas cylinders, analyze the safety of titanium alloy high-pressure gas cylinders under low-temperature conditions, provide a basis for gas cylinder selection, and ensure safety in actual use. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic flow chart of the safety testing method of the titanium alloy high-pressure gas cylinder of the present invention;

[0029] Figure 2 It is a schematic diagram of the structure of the test device for low-temperature fracture toughness test in the present invention.

[0030] Numbers in the figure:

[0031] 10. Container; 10a. Low-temperature tank; 20. Lower support member; 30. Extensometer; 40. Loading device; 41. First loading member; 42. Second loading member; 50. Test specimen; 60. Load sensor; 70. Connecting column; 80. Insulation filler. DETAILED DESCRIPTION

[0032] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific embodiments of the present invention are now described in detail with reference to the accompanying drawings. In the following description, it should be understood that the directions or positional relationships indicated by "front", "back", "up", "down", "left", "right", "longitudinal", "horizontal", "vertical", "horizontal", "top", "bottom", "inside", "outside", "head", "tail", etc. are based on the directions or positional relationships shown in the accompanying drawings, are constructed and operated in a specific direction, and are only for the convenience of describing the present technical solution, rather than indicating that the device or element referred to must have a specific direction, and therefore cannot be understood as a limitation to the present invention.

[0033] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0034] The present application provides a method for testing the safety of a titanium alloy high-pressure gas cylinder, the method comprising:

[0035] S100. Prepare a titanium alloy high-pressure gas cylinder test piece to be tested, wherein the test piece includes a three-point bending specimen cut from a titanium alloy high-pressure gas cylinder pipe and a titanium alloy high-pressure gas cylinder prototype;

[0036] Exemplarily, the preparation of test pieces to be tested needs to be determined according to the type of test to be performed. In this embodiment, in order to evaluate the safety performance of titanium alloy high-pressure gas cylinders and to verify the safety of use of titanium alloy high-pressure gas cylinders in marine environments, two types of test pieces are prepared, namely three-point bending specimens and gas cylinder prototypes.

[0037] In this embodiment, three groups of three-point bending specimens are taken longitudinally and transversely from the titanium alloy high-pressure gas cylinder pipe, with three pieces in each group. The span of the specimen is equal to four times the width, and the ratio of the initial width to the initial thickness of the specimen satisfies the following relationship:

[0038]

[0039] in, - initial thickness of the specimen, - Initial width of the specimen.

[0040] According to the above requirements, the size, shape and surface of the sample are processed to ensure that there are no scratches, damage and rust on the surface to ensure the accuracy of the test. At the same time, prepare a titanium alloy high-pressure gas cylinder prototype.

[0041] S200, conduct low temperature fracture toughness test on the sample, including:

[0042] S201. Prefabricate fatigue cracks on the specimens by cutting notches on the specimens. The notches are straight through notches with a V-shaped bottom. The width of the notches is controlled within 0.1W. Measure the thickness at least at three equally spaced positions along the expected crack extension line. Take the average of the three measurements as the specimen thickness B. Measure the width at at least three points near the notch. Take the average of the three measurements as the specimen width W.

[0043] At room temperature, a fatigue recording method is used to generate a crack at the notch tip of the specimen. The preset crack length satisfies:

[0044]

[0045] S202, injecting liquid cooling medium into the low temperature tank, and continuously adding liquid nitrogen into the liquid cooling medium for stirring; continuously detecting the liquid cooling medium in the low temperature tank by using a temperature detection component until the temperature reaches a preset test temperature, then stopping adding liquid nitrogen and keeping the temperature, and placing the three-point bending specimen prepared in S201 into the low temperature tank.

[0046] Exemplarily, the liquid cooling medium may be anhydrous ethanol, or other liquid commonly used in low-temperature fracture toughness tests in the prior art, without limitation thereto.

[0047] The titanium alloy high-pressure gas cylinder in this embodiment is used in the marine environment. According to the principles of thermodynamics, for general compressible gases, an endothermic effect will occur after throttling expansion, that is, leakage in the high-pressure gas cylinder will cause the temperature of the titanium alloy material to drop. However, since the mass of seawater is infinite relative to the mass of the high-pressure gas cylinder, the leakage of the high-pressure gas cylinder in the seawater will not cause the temperature of the titanium alloy material to drop. The test temperature of the low-temperature fracture toughness test in this embodiment mainly depends on the temperature of the titanium alloy high-pressure gas cylinder when it is above the water surface and leaks.

[0048] Among them, the critical pressure ratio of general compressible gas flow is 0.5283, and the pressure ratio of titanium alloy high-pressure gas cylinder leakage is 0.0025 (external pressure 1 bar / internal pressure 400 bar). The critical state temperature of the gas can be calculated using the one-dimensional isentropic flow principle, and the gas temperature is equivalent to the cylinder material temperature. The calculation formula is as follows:

[0049]

[0050] Where: T0-gas initial temperature, unit is K; γ-adiabatic index; T cr-The temperature at which the gas reaches the critical state, in K. In general, the ambient temperature of the ocean is set at 20°C. Under normal operating conditions of the submarine, the lowest ambient temperature outside the pressure hull (i.e. above the waterline) is -28°C, the highest ambient temperature is 65°C, and the adiabatic index is 1.4. Substituting the above three temperatures into the calculation formula in turn, the material temperatures of the titanium alloy high-pressure gas cylinders under the three environments are: -28.9°C, -68.8°C, and 8.6°C. Therefore, according to the above calculation and analysis, it can be concluded that the theoretical low-temperature environment of titanium alloy materials used in the marine environment is between -28.9°C and -68.8°C. Accordingly, the test temperature of the low-temperature fracture toughness test is set to -30°C to -70°C.

[0051] For example, in order to facilitate understanding of the temperature adjustment of the liquid cooling medium in the low temperature tank, the test temperature of the low temperature fracture toughness test is set to -30°C, -50°C and -70°C as an example for explanation, and the specific temperature adjustment is as follows:

[0052] Anhydrous ethanol is injected into the low temperature tank, and then liquid nitrogen is added to the anhydrous ethanol and stirred. After the temperature detection component detects that the temperature of the anhydrous ethanol reaches -30°C and keeps warm, the first group of samples are placed in the low temperature tank for the first group of low temperature toughness tests; after the first group of tests are completed, liquid nitrogen is continued to be added to the anhydrous ethanol and stirred continuously until the temperature detection component detects that the temperature of the anhydrous ethanol reaches -50°C, then the addition of liquid nitrogen is stopped and kept warm, and the second group of samples are placed in the low temperature tank for the second group of low temperature toughness tests; after the second group of tests are completed, liquid nitrogen is continued to be heated in the anhydrous ethanol and stirred continuously until the temperature detection component detects that the temperature of the anhydrous ethanol reaches -70°C and keeps warm, and the third group of samples are placed in the low temperature tank for the third group of low temperature toughness tests. In this way, the test temperature is quickly adjusted, the cooling time is effectively saved, and it is conducive to improving the test efficiency.

[0053] S203, applying a three-point load to the three-point bending specimen placed in the low-temperature tank in S202, by setting a lower support in the low-temperature tank, placing the three-point bending test specimen in the low-temperature tank and supporting the middle part of the lower surface of the specimen by the lower support, and applying an upward load (i.e., a first point load) to the lower support by a testing machine;

[0054] An extensometer is arranged at the notch position of the specimen to output the precisely positioned relative displacement on both sides of the notch; a first loading member and a second loading member are respectively arranged on both sides of the extensometer, and the first loading member and the second loading member are used to apply an equal force vertically downward to the upper surface of the test piece (i.e., a second point load and a third point load, respectively).

[0055] The height of the lower support is less than the depth of the low-temperature tank, ensuring that the sample can always be in the preset low-temperature environment during the test. The loading rate of the load is controlled at 1mm / min to ensure the safety and reliability of the test process.

[0056] S204. Record the load value. After the specimen breaks, measure the crack length at positions B / 4, B / 2 and 3B / 4. Take the average value of the three positions as the crack length a and calculate the low-temperature fracture toughness of the titanium alloy high-pressure gas cylinder material. , through low temperature fracture toughness The critical crack size of the gas cylinder under low temperature is calculated to provide a basis for the safety analysis of the use of titanium alloy high-pressure gas cylinders under low temperature conditions.

[0057] Low temperature fracture toughness The following relationship should be satisfied:

[0058]

[0059] in:

[0060]

[0061] Where: is the load value, in kN;

[0062] is the thickness of the bending specimen, in cm;

[0063] is the width of the bending specimen, in cm;

[0064] is the crack length, in cm;

[0065] is the span of the bending specimen, in cm.

[0066] It should be noted that the notch in this embodiment may also be a mountain-shaped notch, and there is no limitation on this. However, if a straight-through notch with a V-shaped bottom is used, the root radius of the notch should not be greater than 0.1 mm; if a mountain-shaped notch is used, the root radius of the notch should not be greater than 0.25 mm.

[0067] In one embodiment, a low-temperature fracture toughness test is carried out on a test device, wherein the test device includes a container 10, a lower support member 20, an extensometer 30, a connecting column 70 and a loading device 40, wherein the interior of the container 10 defines a low-temperature tank 10a for accommodating a liquid cooling medium; the lower support member 20 is disposed in the low-temperature tank 10a and is located in the middle of the low-temperature tank 10a; the extensometer 30 is disposed at the crack notch position of the specimen 50; one end of the connecting column 70 passes through the bottom of the container 10 and is connected to the lower support member 20, and the other end of the connecting column 70 is connected to a load sensor 60, which is connected to a testing machine; the loading device 40 includes a first loading member 41 and a second loading member 42 respectively disposed on both sides of the extensometer 30, and the first loading member 41 and the second loading member 42 are used to apply an equal force in a vertical direction to the upper surface of the test piece 50.

[0068] Exemplarily, after the sample 50 is placed into the low-temperature tank 10a, the middle part of the lower surface of the sample 50 is supported by the lower support member 20, and then the first loading member 41 and the second loading member 42 in the loading device 40 are used to apply the same force in the vertical direction to the upper surface of the sample 50, so that the sample 50 is bent at three points and broken, and the fracture toughness of the titanium alloy high-pressure gas cylinder material is calculated based on the data recorded during the test.

[0069] In one embodiment, the container 10 has an inner cavity filled with a heat-insulating filler 80. It should be noted that the heat-insulating filler 80 is made of perlite material so as to insulate the liquid cooling medium in the low-temperature tank and avoid temperature drop during the test, which affects the accuracy of the test.

[0070] S300, Conduct cylinder fatigue test on titanium alloy high pressure cylinder prototype, including:

[0071] S301. Conduct wall thickness measurement, internal and external appearance inspection, surface penetration inspection, and ultrasonic flaw detection on the titanium alloy high-pressure gas cylinder prototype to ensure that the gas cylinder has no obvious defects. If the high-pressure gas cylinder meets the requirements, prefabricate cracks along the axial extension direction in the middle of the outer surface of the cylinder prototype to complete the prefabrication crack treatment of the titanium alloy high-pressure gas cylinder prototype;

[0072] S302. Set a plurality of strain gauges around the prefabricated crack, connect the strain gauges to the strain tester, and perform strain testing through step-up and step-down cycles. Specifically, arrange 4 measuring points around the prefabricated crack and set three-dimensional strain gauges, arrange 2 measuring points on the surface of the gas cylinder far away from the prefabricated crack and set two-dimensional strain gauges; the strain test includes three step-up and step-down cycles, namely, a first training cycle, a second training cycle and a measurement cycle, the maximum pressure of the measurement cycle> the maximum pressure of the second training cycle> the maximum pressure of the first training cycle, the maximum pressure of the measurement cycle is selected according to the pressure environment of the submarine to ensure the accuracy and effectiveness of the strain test, and the principal stress of the measured strain is calculated according to the measuring points.

[0073] S303. Perform hydraulic cyclic fatigue test on the titanium alloy high-pressure gas cylinder prototype by using hydraulic fatigue test equipment. Apply trapezoidal wave load to the titanium alloy high-pressure gas cylinder prototype according to the principal stress level. In this embodiment, the test pressure value is between 3Mpa and 50Mpa, the test frequency is <5 times / minute, the machine is shut down after every 50 fatigue cycles, and the size, depth and direction of prefabricated cracks are detected by using acoustic waves. The fatigue test is continued until the set number of fatigue cycles is reached or the gas cylinder fails. The final gas cylinder failure mode of "leakage without explosion" and no obvious deformation at the rupture are used as the qualification criteria.

[0074] S400, analyze the safety of titanium alloy high-pressure gas cylinders based on low-temperature fracture toughness and whether the high-pressure gas cylinder prototype explodes and has obvious deformation. The critical crack size of the gas cylinder under low temperature is calculated to provide a basis for the safety analysis of the use of titanium alloy high-pressure gas cylinders under low-temperature conditions. The final gas cylinder failure mode of "leakage but no explosion" and no obvious deformation at the crack are used as the safety qualification criteria for titanium alloy high-pressure gas cylinders.

[0075] In one embodiment, the steps of using an acoustic wave emission detection device to perform acoustic wave emission detection on the size, depth and direction of prefabricated cracks on a high-pressure gas cylinder prototype include: emitting sound waves to the high-pressure gas cylinder sample; capturing reflected sound waves by an acoustic wave sensor of the acoustic wave emission detection device, and converting the reflected sound waves into weak electrical signals; amplifying the electrical signals by an amplifier of the acoustic wave emission detection device; processing the amplified signals by a signal processor of the acoustic wave emission detection device, and outputting the processed data.

[0076] Exemplarily, sound waves are emitted to the high-pressure gas cylinder sample, and then the reflected sound waves are captured by the sound wave sensor and converted into weak electrical signals. The electrical signals are then amplified by the amplifier and transmitted to the signal processor for processing, and finally the size, depth, direction, etc. of the crack are output.

[0077] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.

Claims

1. A safety test method for titanium alloy high-pressure gas cylinders, characterized in that: include: Preparing a titanium alloy high-pressure gas cylinder test piece to be tested, wherein the test piece comprises a three-point bending specimen cut from a titanium alloy high-pressure gas cylinder pipe and a titanium alloy high-pressure gas cylinder prototype; Performing a low-temperature fracture toughness test on the sample, wherein the low-temperature fracture toughness test includes prefabricating a fatigue crack on the sample, placing the sample in a preset low-temperature environment, applying a load to the sample, and calculating the low-temperature fracture toughness after the sample is fractured; A cylinder fatigue test is performed on the titanium alloy high-pressure gas cylinder prototype, wherein the cylinder fatigue test includes prefabricating the cylinder prototype with cracks, arranging a plurality of strain gauges around the prefabricated cracks, performing strain testing through pressure increase and decrease cycles, and performing a hydraulic cycle fatigue test through a hydraulic fatigue test device; The safety of the titanium alloy high-pressure gas cylinder is judged based on the low-temperature fracture toughness, whether the high-pressure gas cylinder prototype explodes, and whether there is obvious deformation.

2. The titanium alloy high pressure gas cylinder safety testing method according to claim 1, characterized in that: The three-point bending specimens cut include three-point bending specimens cut in the longitudinal direction and in the transverse direction respectively according to a preset ratio of width to thickness.

3. The titanium alloy high-pressure gas cylinder safety testing method according to claim 2, placing the sample in a preset low-temperature environment comprises: Inject a liquid cooling medium into the low-temperature tank, and continuously add liquid nitrogen into the liquid cooling medium for stirring; continuously detect the liquid cooling medium in the low-temperature tank using a temperature detection component until the temperature reaches a preset test temperature, then stop adding liquid nitrogen and keep the temperature, and place the three-point bending specimen into the low-temperature tank.

4. The titanium alloy high pressure gas cylinder safety testing method according to claim 2, characterized in that: Prefabricating fatigue cracks on the sample includes: forming a notch in the specimen; The fatigue loading method is used to generate a crack of preset length at the top of the notch. The preset ratio of width to thickness and the length of the preset crack should satisfy the following relationship: Where: - initial thickness of the specimen, - initial width of the specimen, L - length of the intended crack, - Width of specimen.

5. The titanium alloy high pressure gas cylinder safety testing method according to claim 4 is characterized in that: Applying a load to the sample comprises: A lower support is arranged in the low-temperature tank, the sample is placed in the low-temperature tank and the lower support supports the middle part of the lower surface of the sample, and an upward load is applied to the lower support by a testing machine; An extensometer is arranged at the notch position of the specimen to output the relative displacement of the two sides of the notch at a precise location; A first loading member and a second loading member are respectively arranged on both sides of the extensometer, and the first loading member and the second loading member are used to apply an equal vertical downward force to the upper surface of the sample.

6. The titanium alloy high pressure gas cylinder safety testing method according to claim 5, characterized in that: The height of the lower support member is less than the depth of the low-temperature tank, and the rate of applying the load to the sample is 1 mm / min.

7. The titanium alloy high pressure gas cylinder safety testing method according to claim 1, characterized in that: The prefabrication crack treatment of the gas cylinder prototype includes prefabrication of axial cracks on the outer surface of the middle part of the prototype bottle body.

8. The titanium alloy high pressure gas cylinder safety testing method according to claim 1 or 7, characterized in that: The method of setting a plurality of strain gauges around the prefabricated crack and performing strain testing by pressure-boosting cycles includes: arranging four measuring points around the prefabricated crack to set three-dimensional strain gauges, and arranging two measuring points on the surface of the gas cylinder away from the prefabricated crack to set two-dimensional strain gauges; The strain test includes two training cycles and one measurement cycle, and the maximum pressure of the measurement cycle is greater than the maximum pressure of the training cycle.

9. The titanium alloy high pressure gas cylinder safety testing method according to claim 8, characterized in that: The hydraulic cycle fatigue test performed by the hydraulic fatigue test device comprises: A trapezoidal wave load is applied to the prototype, with a test frequency of <5 times / minute. The machine is stopped after every 50 fatigue cycles, and the size, depth and direction of the prefabricated cracks are detected by using acoustic waves. The fatigue test is continued until the set fatigue times are reached or the gas cylinder fails.

10. The titanium alloy high pressure gas cylinder safety testing method according to claim 8, characterized in that: The pressure value of the hydraulic cycle fatigue test is between 3Mpa and 50Mpa.

Citation Information

Patent Citations

  • Monitoring method for evaluating service life of gas cylinder by fatigue test combining acoustic emission

    CN109187066A

  • Device for testing low-temperature fracture toughness of material through liquid medium cooling

    CN217212005U

  • Evaluation method for remaining life of pressure vessel

    JP2023158383A