A method for swelling seed microspheres and resin microspheres prepared therefrom and their application
Through the two-step seed swelling polymerization method, styrene divinylbenzene resin microspheres with high crosslinking degree and uniform particle size were prepared, which solved the poor pressure resistance and poor reproducibility of resin microspheres in the prior art. Problem, suitable for chromatographic column fillers.
Patent Information
- Application Number
- CN202410372746.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-29
AI Technical Summary
The existing seed swelling method is difficult to prepare styrene divinylbenzene resin microspheres with high crosslinking and uniform particle size, resulting in poor pressure resistance and poor reproducibility of resin microspheres, making it difficult to meet the chromatographic column filler. Require.
Using a two-step seed swelling polymerization method, the seed microspheres are dried and suitable emulsifiers, pore-generating agents and initiators are added and reacted in batches, and the temperature and stirring conditions are controlled to ensure that the particle size of the resin microspheres is 4- 9 microns and crosslinking degree is between 30-45%.
The particle size uniformity and crosslinking degree of resin microspheres are achieved while improving, and the product's reproducibility and pressure resistance are improved. It is suitable for chromatographic column fillers.
Smart Images

Figure CN118373932B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a seed microsphere and a resin microsphere, and also provides the seed microsphere, a swelling method and application of the seed microsphere. Background Art
[0002] Porous polymer microspheres are widely used in the fields of chromatographic column fillers, ion exchange resins, bioseparation and catalyst carriers. Taking micron-sized styrene divinylbenzene resin microspheres as an example, micron-sized styrene divinylbenzene resin microspheres are a new type of functional material with the advantages of good sphericity, large specific surface area, and easy surface modification. They are one of the available fillers for chromatographic columns such as ion chromatography and liquid chromatography. When used as chromatographic column fillers, the cross-linking degree and particle size uniformity of the resin microspheres are important factors affecting their chromatographic separation effect. The cross-linking degree is required to be at least not less than 25%. A higher cross-linking degree can ensure that the resin microspheres are not easy to swell and dissolve in organic matter, and can withstand greater pressure; and generally a larger particle size (usually 4 to 10 microns) needs to be selected.
[0003] There are many methods for preparing micron-sized styrene divinylbenzene resin microspheres, such as suspension polymerization, dispersion polymerization, seed swelling polymerization and SPG membrane emulsification method, etc. Among them, the seed swelling method is one of the more commonly used methods for preparing monodisperse porous polymer microspheres.
[0004] The seed swelling method prepares seed microspheres (also called seed templates) by emulsion polymerization, soap-free emulsion polymerization or dispersion polymerization, and then introduces an inert solvent and a monomer to swell the monodisperse seed microspheres to prepare monodisperse porous polymer microspheres. However, the existing seed swelling method usually has the following problems when preparing micron-sized styrene divinylbenzene resin microspheres:
[0005] First, during the preparation process, if the prepared resin microspheres are expected to have a particle size suitable for use as chromatographic column fillers or have relatively good uniformity, the prepared resin microspheres usually have a problem of too low cross-linking (generally less than 10%). When the cross-linking is too low, the resin microspheres will have more internal pores, which may bring a large specific surface area, but will make the resin microspheres have poor pressure resistance and easy to collapse;
[0006] For example, the patent application document with application number 201110230790.9 discloses a method for preparing monodisperse microspheres of vinylpyrrolidone and divinylbenzene - a swelling copolymerization method, in which polystyrene microsphere seeds are prepared by dispersion polymerization, and comonomers such as N-vinylpyrrolidone and acrylic acid are introduced during the swelling copolymerization process to prepare corresponding copolymer microspheres.
[0007] The preparation process of this method has the following problems: (1) The solution addition time is relatively long (2-11h), and the solution added during this process may solidify or react prematurely, and deteriorate. In addition, the operation is inconvenient and difficult to control. (2) The aforementioned problem of difficult control of operability will also affect the stability of product properties under the same conditions in different batches, that is, the reproducibility of the microspheres prepared by this method is poor. (3) The particle size of the microspheres synthesized by this method is concentrated between 20-80μm, and the degree of cross-linking is not high enough, which is difficult to meet the requirements of chromatographic fillers.
[0008] Secondly, during the preparation process, if it is desired that the prepared resin microspheres have a higher degree of crosslinking, the particle size of the resin will gradually increase as the degree of crosslinking increases, and the particle size dispersion of the resin will increase, resulting in poor uniformity.
[0009] Therefore, the preparation of porous polymer microspheres with high cross-linking degree, controllable particle size and uniform particle size has great research value and application prospects. Summary of the invention
[0010] 1. Problem to be solved
[0011] Based on the existing preparation methods of porous polymer microspheres, it is impossible to prepare porous polymer microspheres with high crosslinking degree and uniform particle size. One of the purposes of the present invention is to provide a swelling method for seed microspheres. By adopting a two-step seed swelling polymerization method, the particle size uniformity and crosslinking degree of the obtained product can be improved at the same time.
[0012] Based on one of the purposes of the present invention, the present invention also provides resin microspheres and particle groups thereof, as well as chromatographic fillers and chromatographic columns based on the resin microsphere particle groups.
[0013] 2. Technical solution
[0014] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0015] According to the purpose of the present invention, the first aspect of the present invention provides a swelling method for seed microspheres, comprising the following steps:
[0016] S1 prepares raw materials for phase 3:
[0017] The raw material phase three includes seed microspheres and an emulsifier; the seed microspheres are polystyrene microspheres;
[0018] Wherein, the seed microspheres are dried before use, the drying temperature does not exceed 50°C, and the drying time does not exceed 20 minutes;
[0019] S2 Prepare raw materials for phase 4:
[0020] The prepared raw material phase 4 includes styrene, divinylbenzene, porogen, emulsifier, and initiator;
[0021] Wherein, styrene, divinylbenzene, a porogen, and an emulsifier are first mixed, and ultrasonic treatment, stirring, and ultrasonic treatment are performed in sequence, and then an initiator is added and mixed to obtain the raw material phase 4;
[0022] S3 seed microsphere swelling:
[0023] Adding, swelling and reacting the raw material phase 3 and the raw material phase 4;
[0024] The adding is performed in N times, where N is an integer ≥2.
[0025] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, in S2, the raw material phase four includes a first raw material phase four and a second raw material phase four;
[0026] The first raw material phase IV comprises styrene, divinylbenzene, a porogen, an emulsifier, and an initiator; wherein styrene, divinylbenzene, a porogen, and an emulsifier are first mixed, and then ultrasonicated, stirred, and ultrasonically treated in sequence, and then the initiator is added and mixed to obtain the first raw material phase IV;
[0027] The second raw material phase four comprises styrene, divinylbenzene, an emulsifier, and an initiator, wherein styrene, divinylbenzene, and an emulsifier are first mixed, and then ultrasonicated, stirred, and ultrasonically treated in sequence, and then the initiator is added and mixed to obtain the second raw material phase four.
[0028] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, in S2, the ultrasonic conditions include: temperature 20-40° C.; time 5-20 min;
[0029] The stirring conditions include: intensity 150-350 r / min; time 3-15 min.
[0030] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, in S1, the seed microspheres are dried before use, and the drying temperature does not exceed 50° C. and the drying time does not exceed 15 min.
[0031] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, in S1, the seed microspheres are dried before use, and the drying temperature does not exceed 50° C. and the drying time does not exceed 10 min.
[0032] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, the emulsifier includes any one or more of sodium dodecylbenzene sulfonate and sodium dodecyl sulfate;
[0033] The initiator includes any one or more of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, benzoyl peroxide, and dibenzoyl peroxide;
[0034] The porogen includes any one or more of linear polystyrene, dibutyl phthalate, toluene, liquid paraffin, and polyvinyl acetate.
[0035] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, in S1, the mass percentages of seed microspheres and emulsifier are (0.5-2): (0.5-1.5).
[0036] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, in S2, the raw material phase 4 is added to the raw material phase 3 in N times;
[0037] The raw material phase four includes a first raw material phase four and a second raw material phase four.
[0038] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, the mass percentages of styrene, divinylbenzene, porogen, emulsifier and initiator in the first raw material phase four are (1.5~3):(1~4):(1~2):(0.5~1.5):(0.5~1.5).
[0039] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, the mass percentages of styrene, divinylbenzene, emulsifier and initiator in the second raw material phase four are (1.5~3):(1~4):(0.5~1.5):(0.5~1.5).
[0040] According to the seed microsphere swelling method of any embodiment of the first aspect of the present invention, the usage ratio of the first raw material phase four to the raw material phase three is (1-2): (1-2).
[0041] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, the usage ratio of the first raw material phase four to the second raw material phase four is (1~2): (1~2).
[0042] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention,
[0043] In S3, the first raw material phase 4 is added first, and the addition is performed in N times, where N is an integer ≥ 2;
[0044] Then, the second raw material phase four is added, and the addition is performed in N times, where N is an integer ≥2.
[0045] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention,
[0046] The process of adding the first raw material phase 4 includes:
[0047] The temperature during the addition does not exceed 50 degrees Celsius (preferably 30-50 degrees Celsius); the interval time between the addition of the previous batch and the addition of the next batch is 10-120 minutes.
[0048] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, in S3, after the addition of the first raw material phase four is completed, swelling is carried out, and then the reaction is carried out at a temperature of 60-80°C for 4-24h; preferably at 65-75°C for 4-24h.
[0049] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, the process of adding the second raw material phase 4 comprises:
[0050] The temperature of each batch of the second raw material phase 4 when added does not exceed 50°C (preferably 30-50°C); the interval time between the addition of the previous batch and the addition of the next batch is 10-120 minutes.
[0051] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, after the previous batch is added, the temperature is raised to 60-80°C (preferably 65-75°C), reacted for 10-120 minutes, and then cooled to no more than 50°C (preferably 30-50°C) before the next batch is added;
[0052] After the addition of the second raw material phase 4 is completed, swelling is carried out, and then the reaction is carried out at 65-75° C. for 4 to 24 hours; preferably, the reaction is carried out at 65-75° C. for 4 to 24 hours.
[0053] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, calculated based on the mass of the first raw material phase four, the mass ratio of the first raw material phase four in each added batch to the total mass of the first raw material phase four is 20-50wt%.
[0054] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, calculated based on the mass of the second raw material phase four, the mass ratio of the second raw material phase four in each added batch to the total mass of the second raw material phase four is 20-50wt%.
[0055] According to the swelling method of seed microspheres of any embodiment of the first aspect of the present invention, the seed microspheres have a particle size of 0.5-3 µm and a polydispersity index of 1-1.2; preferably, the seed microspheres have a polydispersity index of 1.02-1.1.
[0056] The seed microspheres are prepared by [a seed microsphere and a preparation method thereof].
[0057] Based on the first aspect of the purpose of the present invention, the second aspect of the present invention provides [a resin microsphere], wherein the resin microsphere is prepared by any of the above methods.
[0058] According to the resin microspheres of any embodiment of the second aspect of the present invention, the particle size of the resin microsphere particles is 4-9µm.
[0059] According to the resin microspheres of any embodiment of the second aspect of the present invention, the particle size of the resin microspheres can be any value taken from any of the following numerical ranges: 4-9 microns, 4-8 microns, 4-7 microns, 4-6 microns, 4-5 microns, 5-9 microns, 5-8 microns, 5-7 microns, 5-6 microns, 6-9 microns, 6-8 microns, 6-7 microns, 7-9 microns, 7-8 microns, 8-9 microns.
[0060] According to the resin microspheres of any embodiment of the second aspect of the present invention, the crosslinking degree of the resin microsphere particles is 30% - 45%.
[0061] According to the resin microspheres of any embodiment of the second aspect of the present invention, the degree of crosslinking of the resin microspheres can be any value within any of the following numerical ranges: 30-45%, 30-40%, 30-35%, 35-45%, 35-40%, 40-45%.
[0062] Based on the first aspect of the purpose of the present invention, the third aspect of the present invention provides [a resin microsphere particle group], and the resin microsphere particle group is prepared by any of the above methods.
[0063] According to the resin microsphere particle group of any embodiment of the third aspect of the present invention, the resin microsphere particle group includes resin microsphere particles with a particle size of 4-9µm, accounting for 92.6~97.3wt%.
[0064] According to the resin microsphere particle group of any embodiment of the third aspect of the present invention, the particle size of the resin microspheres can be any value taken from any of the following numerical ranges: 4~9 microns, 4~8 microns, 4~7 microns, 4~6 microns, 4~5 microns, 5~9 microns, 5~8 microns, 5~7 microns, 5~6 microns, 6~9 microns, 6~8 microns, 6~7 microns, 7~9 microns, 7~8 microns, 8~9 microns.
[0065] According to the resin microsphere particle group of any embodiment of the third aspect of the present invention, the resin microsphere particle group includes resin microsphere particles with a crosslinking degree of 30% - 45%.
[0066] According to the resin microsphere particle group of any embodiment of the third aspect of the present invention, the crosslinking degree of the resin microspheres can be any value within any of the following numerical ranges: 30-45%, 30-40%, 30-35%, 35-45%, 35-40%, 40-45%.
[0067] According to the resin microsphere particle group of any embodiment of the third aspect of the present invention, the polydispersity coefficient of the resin microsphere particles contained in the resin microsphere particle group is 1-1.2, preferably has a polydispersity coefficient of 1.02-1.1.
[0068] According to the resin microsphere particle group of any embodiment of the third aspect of the present invention, the polydispersity coefficient of the resin microsphere particles contained in the resin microsphere particle group can be any value within any of the following numerical ranges: 1-1.2, 1.01-1.1, 1.02-1.09, 1.02-1.07, 1.02-1.05, 1.023-1.035, 1.035-1.045, 1.035-1.055, 1.035-1.065, 1.035-1.075, 1.035-1.085, 1.035-1.097.
[0069] Based on any one of the first to third aspects of the present invention, the fourth aspect of the present invention provides a chromatographic filler, which comprises resin microspheres prepared by any of the above methods; and / or any one of the above resin microsphere particle groups.
[0070] Based on any one of the first to fourth aspects of the present invention, the fifth aspect of the present invention provides a chromatographic column, which comprises resin microspheres prepared by any of the above methods; and / or any one of the above resin microsphere particle groups; and / or, chromatographic filler. BRIEF DESCRIPTION OF THE DRAWINGS
[0071] Figure 1 This is the resin microsphere 6-A prepared in Example 6. DETAILED DESCRIPTION
[0072] The present disclosure may be more easily understood by reference to the following description in conjunction with the accompanying drawings and examples, all of which constitute a part of the present disclosure. It should be understood that the present disclosure is not limited to the specific products, methods, conditions or parameters described and / or shown herein. Further, the terms used herein are only used for the purpose of describing specific embodiments by way of example and are not intended to be limiting unless otherwise stated.
[0073] It should also be understood that, for the sake of clarity, certain features of the present disclosure may be described herein in the context of separate embodiments, but may also be provided in combination with each other in a single embodiment. That is, unless clearly incompatible or specifically not included, each separate embodiment is considered to be combinable with any other embodiment, and the combination is considered to represent another different embodiment. Conversely, for the sake of simplicity, the various features of the present disclosure described in the context of a single embodiment may also be provided individually or in any sub-combination. Finally, although a particular embodiment may be described as part of a series of steps or part of a more general structure, each step or substructure itself may also be considered to be an independent embodiment.
[0074] Unless otherwise indicated, it should be understood that each individual element in a list and each combination of individual elements in the list will be interpreted as a different embodiment. For example, a list of embodiments represented as "A, B, or C" should be interpreted to include embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".
[0075] In the present disclosure, the singular forms of the articles "a," "an," and "the" also include the corresponding plural references, and a reference to a specific value includes at least that specific value unless the context clearly indicates otherwise. Thus, for example, a reference to "a substance" is a reference to at least one of that substance and equivalents thereof.
[0076] The terms including ordinal numbers such as "first" and "second" can be used to explain various components or fluids, but these components and fluids are not limited by these terms. Therefore, without departing from the teachings of the present disclosure, these terms are only used to distinguish the component / fluid from another component / fluid.
[0077] When items are described by using the conjunction terms "... and / or...," etc., the description should be understood to include any one of the associated listed items and all combinations of one or more thereof.
[0078] In general, the use of the term "about" indicates an approximate value that may vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to the values stated in the range includes each value within the range.
[0079] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.
[0080] The method for preparing resin microspheres by swelling seed microspheres of the present invention comprises the following steps:
[0081] S1 prepares raw materials for phase 3:
[0082] The raw material phase three includes seed microspheres and an emulsifier;
[0083] S2 Prepare raw materials for phase 4:
[0084] The prepared raw material phase 4 includes styrene, divinylbenzene, a porogen, an emulsifier, and an initiator.
[0085] S3 seed microsphere swelling:
[0086] Allowing the raw material phase 3 and the raw material phase 4 to undergo an addition and swelling total reaction;
[0087] The adding is performed in N times, where N is an integer ≥2.
[0088] The seed microspheres in the raw material phase are polystyrene seed microspheres, and the source is not particularly limited. They can be prepared according to the prior art or purchased.
[0089] The type of emulsifier in the raw material phase is not particularly limited. For example, any one of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, etc., or any combination thereof can be used as an emulsifier;
[0090] The type of porogen in the raw material phase is not particularly limited. For example, any one of linear polystyrene, dibutyl phthalate, toluene, liquid paraffin, polyvinyl acetate, etc., or any combination thereof can be used as the porogen; and from the perspective of improving the system stability during the reaction, the porogen preferably includes dibutyl phthalate and toluene, but does not include linear polystyrene, liquid paraffin, and polyvinyl acetate.
[0091] Furthermore, in S1, the mass percentages of seed microspheres and emulsifier are calculated as (0.5-2):(0.5-1.5); a more preferred ratio is (0.8-1.6):(0.8-1.2).
[0092] In S2, the mass percentages of seed microspheres, styrene, divinylbenzene, porogen, emulsifier and initiator are (0.5~2):(1.5~3):(1~4):(1~2):(0.5~1.5):(0.5~1.5); a more preferred ratio is (0.8~1.6):(2~2.5):(1.5~3):(1.2~1.8):(0.8~1.2):(0.6~1.2).
[0093] The reference process for preparing the raw material phase 3 in S1 is as follows: weigh a certain amount of prepared seed microspheres, add them to an aqueous solution containing an emulsifier, disperse them ultrasonically, and then stir them evenly. It should be emphasized here that before using the "seed microspheres", they need to be dried at low temperature for a short time (temperature not exceeding 50°C, time not exceeding 20min). On the one hand, it can eliminate the differences in the "different seed microspheres" during storage as much as possible (for example, some seed microspheres have more water content, some seed microspheres have less water content, and the differences between the various seed microspheres formed in this way). On the other hand, it can also eliminate the differences in the internal and external surfaces of the same seed microsphere during storage (for example, the surface of the seed microsphere has more water content, the internal water content is less, and the differences between the internal and external surfaces of the seed microspheres formed in this way) while not changing the properties of the seed microspheres due to the influence of temperature; in addition, the quality accuracy of the seed microspheres can be guaranteed. This operation will affect the crosslinking degree, particle size, and particle size uniformity of the resin microspheres (the resin microsphere particle group) finally prepared.
[0094] The reference process for preparing raw material phase 4 in S2 is as follows: first mix styrene, divinylbenzene, porogen, and emulsifier (or first mix styrene, divinylbenzene, and emulsifier), and perform a dispersion operation; then add an initiator to mix to obtain the raw material phase 4. It should be emphasized here that the sign of the end of the "dispersion operation" is "taking the liquid to observe under a microscope until there are no obvious oil droplets". Based on this, the "dispersion operation" method described herein will have a great impact on the process time. Based on this, from the perspective of reducing the process time, it is preferred to perform the "dispersion operation" in accordance with the "sequential combination of ultrasound, stirring, and ultrasound", which can reduce the process time by nearly 50% (compared to a single ultrasound or a single stirring). Another reference process for preparing raw material phase 4 in S2 based on this is as follows: wherein, first mix styrene, divinylbenzene, porogen, and emulsifier, perform ultrasound, stirring, and ultrasound treatment in sequence, take the liquid to observe under a microscope until there are no obvious oil droplets, and then add an initiator to mix to obtain the raw material phase 4. However, it should be noted that the composition of the system of raw material phase four itself will also affect the time required for the "dispersion operation to achieve the effect of taking the liquid under a microscope and observing it until there are no obvious oil droplets". Therefore, it is summarized that it is recommended that the ultrasonic conditions meet the following points: temperature 20~40℃; time 5~20min; the stirring conditions include: intensity 150~350r / min; time 3~15min. In this case, for the object of the same "dispersion operation", performing the "dispersion operation" in accordance with the "sequential combination of ultrasound, stirring, and ultrasound" can reduce the process time by nearly 50% (compared to single ultrasound, or single stirring), such as the preparation time of the following resin microspheres 6-A and comparison sample-6.
[0095] The reference process for swelling the S3 seed microspheres is as follows: add the raw material phase 4 prepared in step S2 into the raw material phase 3 prepared in step S1 in N batches. During the addition of each batch of raw material phase 4 to raw material phase 3, the temperature must be maintained at 30-50°C, accompanied by stirring;
[0096] Calculated according to the mass of the raw material phase 4, the mass ratio of the raw material phase 4 in each batch to the total amount of the raw material phase 4 is 20-50wt%; the interval time between the addition of the previous batch and the addition of the next batch is 10-120min.
[0097] After all batches of raw materials in phase 4 are added, the temperature is raised (the heating rate does not exceed 10°C / h) to 60-80 degrees Celsius, and the reaction is carried out at 60-80 degrees Celsius for 4-24 hours. After the reaction, the porogen is removed by ultrasonic washing, centrifugation, and Soxhlet extraction to obtain the final resin microspheres.
[0098] While simultaneously considering the pursuit of the uniformity of the particle size and the degree of crosslinking of the resin microspheres finally obtained, the reference process for preparing the raw material phase 4 in S2 is as follows:
[0099] dividing the raw material phase 4 into a first raw material phase 4 and a second raw material phase 4; and,
[0100] The amount ratio of the first raw material phase 4 to the raw material phase 3 is (1-2): (1-2);
[0101] The usage ratio of the first raw material phase 4 to the second raw material phase 4 is (1-2): (1-2).
[0102] As the first raw material phase four, it includes styrene, divinylbenzene, a porogen, an emulsifier, and an initiator, and the mass percentages of the styrene, divinylbenzene, a porogen, an emulsifier, and an initiator are (1.5-3): (1-4): (1-2): (0.5-1.5): (0.5-1.5);
[0103] As the second raw material phase four, it includes styrene, divinylbenzene, an emulsifier, and an initiator. The mass percentages of styrene, divinylbenzene, emulsifier, and initiator are (1.5~3):(1~4):(0.5~1.5):(0.5~1.5).
[0104] Furthermore, based on the above-mentioned S2 preparation of raw materials phase 4, another reference process for S3 seed microsphere swelling is as follows:
[0105] The first raw material phase 4 prepared in step S2 is added to the raw material phase 3 prepared in step S1 in N batches. During the addition of each batch of the first raw material phase 4 to the raw material phase 3, the temperature must be maintained at no more than 50° C., and stirring is performed during the process;
[0106] Calculated according to the mass of the first raw material phase 4, the mass ratio of the first raw material phase 4 in each batch to the total mass of the first raw material phase 4 is 20-50wt%; the interval time between the addition of the previous batch and the addition of the next batch is 10-120min.
[0107] After all batches of the first raw material phase four are added, keep warm at the addition temperature for 8 to 16 hours, then raise the temperature to 60-80 degrees Celsius, react at 60-80 degrees Celsius for 2 to 4 hours, and then proceed to the second raw material phase four addition stage after the reaction is completed.
[0108] The reference addition process of the second raw material phase 4 is as follows: the second raw material phase 4 prepared in step S2 is added to the raw material phase 3 prepared in step S1 in N batches. During the addition of each batch of the second raw material phase 4 to the raw material phase 3, the temperature must be maintained at 30-50°C, accompanied by stirring;
[0109] The time interval from the completion of adding the second raw material phase 4 of the previous batch to the raw material phase 3 to the start of adding the second raw material phase 4 of the next batch to the raw material phase 3 is 10-120 minutes; and during this time interval, there is a process of heating-keeping-cooling treatment to ensure that the temperature of each batch of the second raw material phase 4 is 30-50°C when adding. This cycle is repeated until all batches of the first raw material phase 4 are added;
[0110] Finally, the temperature is raised (the heating rate does not exceed 10°C / h) to 65-75 degrees Celsius, and the swelling total reaction is carried out at 65-75 degrees Celsius for 4-24 hours; after the reaction, the porogen is removed by ultrasonic washing, centrifugation, and Soxhlet extraction to obtain the final resin microspheres. Finally, the particle size of the prepared resin microspheres is 4-9 µm.
[0111] For the heating-keeping-cooling treatment, the generally referenced heating rate is no more than 10°C / h, for example, the heating rate is 2°C / h, 3°C / h, 4°C / h, 5°C / h, 6°C / h, 7°C / h, 8°C / h, 9°C / h;
[0112] The heat preservation treatment temperature for reference can be any temperature between 65 and 75°C, such as 65°C, 67°C, 70°C, 73°C, etc.
[0113] The insulation treatment time for reference may be any time selected from 5-60 min, for example, 5 min, 8 min, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.
[0114] For example, after the second raw material phase 4 of the previous batch is added at 40°C and kept at 40°C for half an hour, the following heating-keeping-cooling process is performed for reference: increase the temperature to 70°C at a rate of 5°C / h, keep at 70°C for half an hour, and then cool to 40°C.
[0115] After the heating-keeping-cooling process is completed, the next batch of the second raw material phase 4 can be added at 40° C., and the cycle is repeated until the last batch of the second raw material phase 4 is added, and then the temperature is kept at 40° C. for half an hour;
[0116] Finally, the temperature is raised (the heating rate does not exceed 5°C / h) to 70 degrees Celsius, and the total reaction is carried out at 70 degrees Celsius for 4-24 hours. After the reaction is completed, the porogen is removed by ultrasonic washing, centrifugation, and Soxhlet extraction to obtain the final resin microspheres.
[0117] Based on the preparation method provided by the present invention, the present invention can also provide resin microsphere particles or resin microsphere particle groups.
[0118] On the basis of the above method, if the uniformity of the particle size and the effect of the degree of crosslinking of the resin microspheres finally obtained are taken into consideration, the seed microspheres in the raw material phase in the above preparation method preferably have a polydispersity coefficient of 1-1.2, and more preferably, the seed microspheres have a polydispersity coefficient of 1.02-1.1.
[0119] If it is further desired to control the particle size of the final resin microspheres to be in the range of 4 to 10 microns. Then, the particle size of the seed microspheres is preferably 0.5-3 μm. For example, the particle size of the seed microspheres can be any value taken from any of the following numerical ranges: 0.5 to 3 μm, 0.5 to 2.5 μm, 0.5 to 2 μm, 0.5 to 1.5 μm, 0.5 to 1 μm, 1 to 3 μm, 1 to 2.5 μm, 1 to 2 μm, 1 to 1.5 μm, 1.5 to 3 μm, 1.5 to 2.5 μm, 1.5 to 2 μm, 2 to 3 μm, 2 to 2.5 μm, 2.5 to 3 μm.
[0120] Based on the above, the present invention can also provide resin microsphere particles: the particle size of the resin microsphere particles is 4-9 μm; and / or,
[0121] The crosslinking degree of the resin microsphere particles is 30% - 45%. And,
[0122] Based on the above, the present invention can also provide a group of resin microsphere particles: the group of resin microsphere particles includes resin microsphere particles with a particle size of 4-9 μm, accounting for 92.6-97.3wt%; and / or,
[0123] The resin microsphere particle group comprises resin microsphere particles having a crosslinking degree of 30% to 45%; and / or,
[0124] The polydispersity coefficient of the resin microsphere particles contained in the resin microsphere particle group is 1-1.2, and the preferred dispersion coefficient is 1.023-1.097.
[0125] Based on the preparation method provided by the present invention, the present invention can also provide a chromatographic filler: the chromatographic filler comprises resin microsphere particles and / or a group of resin microsphere particles prepared by any of the above methods.
[0126] Based on the preparation method provided by the present invention, the present invention can also provide a chromatographic column: the chromatographic column comprises resin microsphere particles, and / or a group of resin microsphere particles, and / or chromatographic fillers prepared by any of the above methods.
[0127] In order to demonstrate the technical solutions and advantages of the present invention, the technical solutions of the present invention will be fully described below using embodiments.
[0128] Example 1
[0129] Deblocking treatment: After washing styrene and divinylbenzene three times with 1M sodium hydroxide solution, the pH of the washing solution is close to neutral.
[0130] Raw material phase 1: Add 350 mL of ethanol, 100 mL of water, and 100 mL of ethylene glycol methyl ether to a 1000 mL three-necked flask, place in a water bath, maintain the water temperature at 40 degrees Celsius, turn on stirring, and stir at a speed of 200 r / min. After stirring for 5 minutes, weigh 9 g of polyvinyl pyrrolidone and 0.6 g of polyvinyl alcohol (molecular weight of 5000) and add them to the mixed solution;
[0131] Raw material phase 2: Weigh 85g of deblocked styrene into a beaker, then weigh 2.5g of azobisisobutyronitrile and add it to the weighed styrene. Place the beaker in a 50-degree water bath and stir with a glass rod to dissolve the azobisisobutyronitrile;
[0132] Synthesis of seed microspheres (seed balls): Keep the water temperature at 40 degrees Celsius, add the prepared raw material phase 2 into the three-necked flask containing the raw material phase 1, and stir during the process. The stirring speed is 350 r / min. After the addition is completed, keep warm at 40 degrees Celsius for half an hour, then increase the temperature to 45 degrees Celsius, keep warm at 45 degrees Celsius for half an hour, continue to increase the temperature to 50 degrees Celsius, keep warm at 50 degrees Celsius for half an hour, continue to increase the temperature and keep warm (each time the temperature increases by 5 minutes, and then keeps warm for half an hour) until 75 degrees Celsius, and react at 75 degrees Celsius for 20 hours.
[0133] After the reaction, centrifuge and wash three times with ethanol and acetone respectively. The washing process is as follows: after adding ethanol / acetone, ultrasonic dispersion for 5 minutes, and then centrifuge at a speed of 3000 r / min and a centrifugal time of 2 minutes.
[0134] Transfer the washed balls to a watch glass and dry them in an oven at 60°C. Store the dried balls in a ziplock bag to prevent them from absorbing water.
[0135] The average particle size of the prepared seed microspheres (seed microspheres-1) is 1.9 µm, and the polydispersity coefficient is 1.029.
[0136] Example 2
[0137] Deblocking treatment: After washing styrene and divinylbenzene three times with 1M sodium hydroxide solution, the pH of the washing solution is close to neutral.
[0138] Raw material phase 1: Add 350 mL of ethanol, 100 mL of water, and 100 mL of ethylene glycol methyl ether to a 1000 mL three-necked flask, place in a water bath, maintain the water temperature at 40 degrees Celsius, turn on stirring, and stir at a speed of 200 r / min. After stirring for 5 minutes, weigh 7g of polyvinyl pyrrolidone and 1g of polyvinyl alcohol (molecular weight of 5000) and add them to the mixed solution.
[0139] Raw material phase 2: Weigh 85g of deblocked styrene into a beaker, then weigh 2.1g of azobisisobutyronitrile and add it to the weighed styrene. Place the beaker in a 50-degree water bath to dissolve the azobisisobutyronitrile;
[0140] Synthesis of seed microspheres (seed balls): Keep the water temperature at 40 degrees Celsius, add the prepared raw material phase 2 into the three-necked flask containing the raw material phase 1, and stir during the process. The stirring speed is 400 r / min. After the addition is completed, keep warm at 40 degrees Celsius for half an hour, then increase the temperature to 45 degrees Celsius, keep warm at 45 degrees Celsius for half an hour, continue to increase the temperature to 50 degrees Celsius, keep warm at 50 degrees Celsius for half an hour, continue to increase the temperature and keep warm (each time the temperature increases by 5 minutes, and then keeps warm for half an hour) until 75 degrees Celsius, and react at 75 degrees Celsius for 20 hours.
[0141] After the reaction, centrifuge and wash three times with ethanol and acetone respectively. The washing process is as follows: after adding ethanol / acetone, ultrasonic dispersion for 5 minutes, and then centrifuge at a speed of 3000 r / min and a centrifugal time of 2 minutes.
[0142] Transfer the washed balls to a watch glass and dry them in an oven at 60°C. Store the dried balls in a ziplock bag to prevent them from absorbing water.
[0143] The prepared seed microspheres (seed microspheres-2) have a particle size of 2.3 µm and a polydispersity coefficient of 1.039.
[0144] Example 3
[0145] Deblocking treatment:
[0146] After washing styrene and divinylbenzene three times with 1 M sodium hydroxide solution, the pH of the washing solution was close to neutral.
[0147] Raw material phase 1: Add 350 mL of ethanol, 100 mL of water, and 60 mL of ethylene glycol methyl ether to a 1000 mL three-necked flask, place in a water bath, maintain the water temperature at 40 degrees Celsius, turn on stirring, and stir at a speed of 200 r / min. After stirring for 5 minutes, weigh 8 g of polyvinyl pyrrolidone and 0.9 g of hydroxypropyl methylcellulose and add them to the mixed solution.
[0148] Raw material phase 2: Weigh 85g of deblocked styrene into a beaker, then weigh 2.5g of azobisisobutyronitrile and add it to the weighed styrene. Place the beaker in a 50-degree water bath to dissolve the azobisisobutyronitrile;
[0149] Synthesis of seed microspheres (seed balls): Keep the water temperature at 40 degrees Celsius, add the prepared raw material phase 2 into the three-necked flask containing the raw material phase 1, and stir during the process. The stirring speed is 400 r / min. After the addition is completed, keep warm at 40 degrees Celsius for half an hour, then increase the temperature to 45 degrees Celsius, keep warm at 45 degrees Celsius for half an hour, continue to increase the temperature to 50 degrees Celsius, keep warm at 50 degrees Celsius for half an hour, continue to increase the temperature and keep warm (each time the temperature increases by 5 minutes, and then keeps warm for half an hour) until 75 degrees Celsius, and react at 75 degrees Celsius for 20 hours.
[0150] After the reaction, centrifuge and wash three times with ethanol and acetone respectively. The washing process is as follows: after adding ethanol / acetone, ultrasonic dispersion for 5 minutes, and then centrifuge at a speed of 3000 r / min and a centrifugal time of 2 minutes.
[0151] Transfer the washed balls to a watch glass and dry them in an oven at 60°C. Store the dried balls in a ziplock bag to prevent them from absorbing water.
[0152] The prepared seed microspheres (seed microspheres-3) have a particle size of 2.2 µm and a polydispersity coefficient of 1.076.
[0153] Example 4
[0154] Deblocking treatment:
[0155] After washing styrene and divinylbenzene three times with 1 M sodium hydroxide solution, the pH of the washing solution was close to neutral.
[0156] Raw material phase 1: Add 350 mL ethanol, 100 mL water, and 60 mL ethylene glycol methyl ether to a 1000 mL three-necked flask, place in a water bath, maintain the water temperature at 40 degrees Celsius, turn on stirring, and stir at a speed of 200 r / min. After stirring for 5 minutes, weigh 7.5 g polyvinyl alcohol (molecular weight 89000) and 1 g hydroxypropyl methylcellulose and add them to the mixed solution.
[0157] Raw material phase 2: Weigh 85g of deblocked styrene into a beaker, then weigh 2.5g of azobisisobutyronitrile and add it to the weighed styrene. Place the beaker in a 50-degree water bath to dissolve the azobisisobutyronitrile;
[0158] Synthesis of seed microspheres (seed balls): Keep the water temperature at 40 degrees Celsius, add the prepared raw material phase 2 into the three-necked flask containing the raw material phase 1, and stir during the process. The stirring speed is 400 r / min. After the addition is completed, keep warm at 40 degrees Celsius for half an hour, then increase the temperature to 45 degrees Celsius, keep warm at 45 degrees Celsius for half an hour, continue to increase the temperature to 50 degrees Celsius, keep warm at 50 degrees Celsius for half an hour, continue to increase the temperature and keep warm (each time the temperature increases by 5 minutes, and then keeps warm for half an hour) until 75 degrees Celsius, and react at 75 degrees Celsius for 20 hours.
[0159] After the reaction, centrifuge and wash three times with ethanol and acetone respectively. The washing process is as follows: after adding ethanol / acetone, ultrasonic dispersion for 5 minutes, and then centrifuge at a speed of 3000 r / min and a centrifugal time of 2 minutes.
[0160] Transfer the washed balls to a watch glass and dry them in an oven at 60°C. Store the dried balls in a ziplock bag to prevent them from absorbing water.
[0161] The prepared seed microspheres (seed microspheres-4) have a particle size of 1.9 µm and a polydispersity coefficient of 1.091.
[0162] Example 5
[0163] In this example, the seed microspheres prepared in Example 1, i.e., seed microspheres-1, were used to prepare resin microspheres. The specific steps are as follows:
[0164] The bulbs were first dried at 50 degrees Celsius for 10 minutes.
[0165] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 3 g of the ball and add it to the solution.
[0166] Ultrasonicate the three-necked flask for 40 minutes to evenly disperse the bulbs. Place the three-necked flask containing the bulbs in a water bath, maintain the temperature at 40 degrees Celsius, and use mechanical stirring at a speed of 350 r / min.
[0167] Raw material phase 4:
[0168] The first part: weigh 1g sodium dodecyl sulfate and add it to 100mL water, add 4g styrene, 8g divinylbenzene (purity 80%), 2mL dibutyl phthalate, 2mL toluene, perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 1.5g benzoyl peroxide and 0.4g azobisisobutyronitrile, and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30℃; time 10 min; the stirring conditions are: 200r / min; time 10 min.
[0169] The second portion: weigh 0.5g sodium dodecyl sulfate and add it to 50mL water, add 2g styrene, 4g divinylbenzene (purity 80%), perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 0.7g benzoyl peroxide and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30℃; time 10 min; the stirring conditions are: 200r / min; time 10 min.
[0170] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;
[0171] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;
[0172] Then, cool down to 50 degrees Celsius;
[0173] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.
[0174] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.
[0175] After washing with ethanol for several times, the mixture was extracted and dried to constant weight at 50°C. The particle size of the resin microspheres was measured to be 4.3 µm, the polydispersity coefficient was 1.037, and the cross-linking degree was 41%.
[0176] Example 6
[0177] In this example, the seed microspheres prepared in Example 2, i.e., seed microspheres-2, were used to prepare resin microspheres. The specific steps are as follows:
[0178] The bulbs were first dried at 40 degrees Celsius for 15 minutes.
[0179] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 2.5 g of the bulbs and add them to the solution.
[0180] Ultrasonicate the three-necked flask for 40 minutes to evenly disperse the bulbs. Place the three-necked flask containing the bulbs in a water bath, maintain the temperature at 40 degrees Celsius, and use mechanical stirring at a speed of 400 r / min.
[0181] Raw material phase 4:
[0182] The first part: weigh 1g sodium dodecyl sulfonate and add it to 100mL water, add 3.5g styrene, 7g divinylbenzene (purity 65%), 2mL dibutyl phthalate, 2mL toluene, perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 1.2g benzoyl peroxide and 0.3g azobisisobutyronitrile, and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30℃; time 7min; the stirring conditions are: intensity 300 r / min; time 7min.
[0183] The second portion: weigh 0.5 g of sodium dodecyl sulfonate and add it to 50 mL of water, add 1.2 g of styrene, and 2.3 g of divinylbenzene (purity 80%), perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 0.4 g of benzoyl peroxide and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30°C; time 7 min; the stirring conditions are: intensity 300 r / min; time 7 min.
[0184] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;
[0185] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;
[0186] Then, cool down to 50 degrees Celsius;
[0187] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.
[0188] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.
[0189] After washing with ethanol for several times, extraction was performed and drying was performed at 50 degrees Celsius to constant weight to obtain resin microspheres 6-A.
[0190] In addition, the samples of resin microspheres 6-B, 6-C and 6-D were prepared in the same manner as the steps of resin microspheres 6-A. The properties of each batch of samples were stable. The properties of the final samples are shown in Table 1:
[0191] Average particle size µm Polydispersity coefficient Degree of crosslinking Resin microspheres 6-A 5.3 1.046 38% Resin microspheres 6-B 5.5 1.049 37% Resin microspheres 6-C 5.4 1.039 36% Resin microspheres 6-D 5.3 1.043 37%
[0192] Comparative Example
[0193] Comparative sample-5:
[0194] The preparation of raw material phase 3 is the same as in Example 6;
[0195] The preparation of raw material phase 4 is the same as in Example 6;
[0196] Swelling of seed microspheres:
[0197] At 40 degrees Celsius, the first raw material phase 4 was added dropwise to the raw material phase 3 for 5 hours, and then the temperature was raised to 45 degrees Celsius and kept at 45 degrees Celsius for 8 hours;
[0198] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;
[0199] Then, the temperature was lowered to 50 degrees Celsius, and the second portion of the raw material phase 4 was added dropwise for 5 hours, and then kept at 50 degrees Celsius for 5 hours;
[0200] After the swelling was completed, the temperature was raised to 70 degrees Celsius, the reaction was carried out for 5 hours, and the heating was stopped to obtain the resin microsphere comparison sample-5-A.
[0201] In addition, according to the same steps as comparison sample 5-A, comparison sample 5-B, comparison sample 5-C, and comparison sample 5-D were prepared respectively. As shown in Table 2, the properties of each batch of samples are quite different.
[0202] Comparative sample-6:
[0203] The preparation of raw material phase 3 is the same as in Example 6;
[0204] The swelling of the seed microspheres was the same as in Example 6;
[0205] The difference lies in the preparation of the raw materials in phase 4:
[0206] During the preparation of the first raw material phase 4 and the second raw material phase 4, simple ultrasound was used instead of the "sonication, stirring, and ultrasonic treatment" described in Example 6. Finally, the liquid was observed under a microscope until no obvious oil droplets were found.
[0207] In this example, the first raw material phase 4 was ultrasonically treated at a temperature of 30° C. for 47 minutes, and the liquid was observed under a microscope to reach a level without obvious oil droplets; compared with the time of Example 6, the time taken for this step in this example was extended by 26 minutes;
[0208] The second raw material phase 4 was ultrasonically treated at a temperature of 30° C. for 45 minutes, and the liquid was observed under a microscope to reach a level without obvious oil droplets; compared with the time of Example 6, the time consumption of this step in this example was extended by 24 minutes.
[0209] Comparative sample-7:
[0210] The preparation of raw material phase 3 is the same as in Example 6;
[0211] The preparation of raw material phase 4 is the same as in Example 6;
[0212] The swelling of the seed microspheres was the same as in Example 6;
[0213] The only difference is that the bulbs were not dried as shown in Example 6 before use. That is, the bulbs were directly taken out after being dried and stored in a ziplock bag for 7 days in Example 2 to prepare the resin microsphere comparison sample-7.
[0214] The final sample properties are shown in Table 2:
[0215] Average particle size µm Polydispersity coefficient Degree of crosslinking Comparative Sample-5-A 4.6 1.237 36% Comparative Sample-5-B 4.2 1.287 39% Comparative Sample-5-C 3.9 1.209 41% Comparative sample-5-D 5.2 1.346 34% Comparative sample-7 4.5 1.167 35%
[0216] Example 7
[0217] In this example, the seed microspheres prepared in the example, i.e., seed microspheres-3 in Example 3, were used to prepare resin microspheres. The specific steps are as follows:
[0218] The bulbs were first dried at 50 degrees Celsius for 10 minutes.
[0219] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 3 g of the ball and add it to the solution.
[0220] Ultrasonicate the three-necked flask for 40 min to evenly disperse the bulb-3. Place the three-necked flask containing the bulb in a water bath, maintain the temperature at 40 degrees Celsius, and use mechanical stirring at a stirring speed of 350 r / min.
[0221] Raw material phase 4:
[0222] The first part: weigh 1g sodium dodecyl sulfate and add it to 100mL water, add 4g styrene, 8g divinylbenzene (purity 80%), 2mL dibutyl phthalate, 2mL toluene, perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 1.5g benzoyl peroxide and 0.4g azobisisobutyronitrile, and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30℃; time 10min; the stirring conditions are: intensity 250r / min; time 8min.
[0223] The second part: weigh 0.5g sodium dodecyl sulfate and add it to 50mL water, add 2g styrene, 4g divinylbenzene (purity 80%), perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 0.7g benzoyl peroxide and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30℃; time 10min; the stirring conditions are: intensity 250r / min; time 8min.
[0224] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;
[0225] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;
[0226] Then, cool down to 50 degrees Celsius;
[0227] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.
[0228] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.
[0229] After washing with ethanol for several times, the mixture was extracted and dried to constant weight at 50°C. The particle size of the resin microspheres was measured to be 4.8 µm, the polydispersity coefficient was 1.113, and the cross-linking degree was 39%.
[0230] Example 8
[0231] In this example, the seed microspheres prepared in the example, i.e., seed microspheres-4 of Example 4, were used to prepare resin microspheres. The specific steps are as follows:
[0232] The bulbs were first dried at 50 degrees Celsius for 10 minutes.
[0233] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 3 g of the ball and add it to the solution.
[0234] Ultrasonicate the three-necked flask for 40 min to evenly disperse the bulb-4. Place the three-necked flask containing the bulb in a water bath, maintain the temperature at 40 degrees Celsius, and use mechanical stirring at a stirring speed of 350 r / min.
[0235] Raw material phase 4:
[0236] The first part: weigh 1g sodium dodecyl sulfate and add it to 100mL water, add 4g styrene, 8g divinylbenzene (purity 80%), 2mL dibutyl phthalate, 2mL toluene, perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 1.5g benzoyl peroxide and 0.4g azobisisobutyronitrile, and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30℃; time 10min; the stirring conditions are: intensity 300r / min; time 6min.
[0237] The second part: weigh 0.5g sodium dodecyl sulfate and add it to 50mL water, add 2g styrene, 4g divinylbenzene (purity 80%), perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 0.7g benzoyl peroxide and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30℃; time 10min; the stirring conditions are: intensity 300r / min; time 6min.
[0238] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;
[0239] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;
[0240] Then, cool down to 50 degrees Celsius;
[0241] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.
[0242] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.
[0243] After washing with ethanol for several times, the mixture was extracted and dried to constant weight at 50°C. The particle size of the resin microspheres was measured to be 4.3 µm, the polydispersity coefficient was 1.127, and the cross-linking degree was 36%.
[0244] Example 9
[0245] In this example, the seed microspheres prepared in Example 1, i.e., seed microspheres-1, were used to prepare resin microspheres. The specific steps are as follows:
[0246] The bulbs were first dried at 50 degrees Celsius for 10 minutes.
[0247] Raw material phase 3: Add 150 mL ultrapure water to a 500 mL three-necked flask, weigh 1.5 g sodium dodecyl sulfonate and add it to the water, turn on the stirring at a speed of 200 r / min. After the sodium dodecylbenzene sulfonate is dissolved, weigh 3 g of the ball and add it to the solution.
[0248] Ultrasonicate the three-necked flask for 40 minutes to evenly disperse the bulbs. Place the three-necked flask containing the bulbs in a water bath, maintain the temperature at 40 degrees Celsius, and use mechanical stirring at a speed of 350 r / min.
[0249] Raw material phase 4:
[0250] The first part: weigh 1g sodium dodecyl sulfate and add it to 100mL water, add 4g styrene, 9g divinylbenzene (purity 80%), 2.5mL dibutyl phthalate, 2mL toluene, perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 1.5g benzoyl peroxide and 0.4g azobisisobutyronitrile, and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30℃; time 8min; the stirring conditions are: intensity 300r / min; time 8min.
[0251] The second part: weigh 0.5g sodium dodecyl sulfate and add it to 50mL water, add 2g styrene, 4.5g divinylbenzene (purity 80%), perform ultrasonic treatment, stirring, and ultrasonic treatment in sequence, take the liquid and observe it under a microscope until there are no obvious oil drops, then add 0.7g benzoyl peroxide and disperse it evenly by ultrasonic treatment. The ultrasonic conditions are: temperature 30℃; time 8min; the stirring conditions are: intensity 300r / min; time 8min.
[0252] Swelling of seed microspheres: add 40 mL of the first raw material phase 4 to the raw material phase 3, stir for 10 minutes, then add 30 mL of the first raw material phase 4 to the raw material phase 3, stir for half an hour, then add the remaining 30 mL of the first raw material phase 4 and swell for 12 hours;
[0253] After the swelling is completed, the temperature is raised to 70 degrees Celsius and the reaction is carried out for 2 hours;
[0254] Then, cool down to 50 degrees Celsius;
[0255] Continue to add 20 mL of the second raw material phase four, stir at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; then lower the temperature to 50 degrees Celsius, add 10 mL of the second raw material phase four, maintain at 50 degrees Celsius for 10 minutes, then raise the temperature to 70 degrees Celsius and react for half an hour; repeat the above process until the addition of raw material phase four is complete.
[0256] After the addition of raw material phase 4 is completed, the temperature is raised to 70 degrees Celsius, the reaction is carried out for 10 hours, and the heating is stopped.
[0257] After washing with ethanol for several times, the mixture was extracted and dried to constant weight at 50°C. The particle size of the resin microspheres was measured to be 4.1 µm, the polydispersity coefficient was 1.046, and the cross-linking degree was 43%.
Claims
1. A method for swelling seed microspheres, characterized in that: The following steps are involved: S1 prepares raw materials for phase 3: The raw material phase three includes seed microspheres and an emulsifier; the mass percentage of the seed microspheres and the emulsifier is (0.5-2): (0.5-1.5); Wherein, the seed microspheres are dried before use, the drying temperature does not exceed 50°C, and the drying time does not exceed 20 minutes; S2 Prepare raw materials for phase 4: The raw material phase 4 includes a first raw material phase 4 and a second raw material phase 4; The first raw material phase IV comprises styrene, divinylbenzene, a porogen, an emulsifier, and an initiator; wherein styrene, divinylbenzene, a porogen, and an emulsifier are first mixed, and then ultrasonicated, stirred, and ultrasonically treated in sequence, and then the initiator is added and mixed to obtain the first raw material phase IV; The second raw material phase IV comprises styrene, divinylbenzene, an emulsifier, and an initiator, wherein styrene, divinylbenzene, and an emulsifier are first mixed, and then ultrasonicated, stirred, and ultrasonically treated in sequence, and then the initiator is added and mixed to obtain the second raw material phase IV; S3 seed microsphere swelling: The raw material phase 3 and the raw material phase 4 are added, swelled, and reacted; the adding includes: firstly adding the first raw material phase 4, the adding is performed in N times, and N is an integer ≥ 2; after the first raw material phase 4 is added, the second raw material phase 4 is added; the second raw material phase 4 is added in N times, and N is an integer ≥ 2; When adding the first raw material phase 4, the temperature does not exceed 50° C., and the interval between the previous batch addition and the next batch addition is 10-120 minutes; after the first raw material phase 4 is added, swelling is performed, and then the reaction is performed at a temperature of 60-80° C. for 4-24 hours; When adding the second raw material phase four, the temperature does not exceed 50°C, and the interval time between the previous batch addition and the next batch addition is 10-120min; after the previous batch is added, the temperature is raised to 65-75°C, reacted for 10~120min, and then cooled to no more than 50°C before the next batch is added; after the second raw material phase four is added, swelling is carried out, and then the reaction is carried out at a temperature of 60-80°C for 4~24h.
2. The method for swelling seed microspheres according to claim 1, characterized in that: In S3, the raw material phase 4 is added to the raw material phase 3 in N times; The raw material phase 4 includes a first raw material phase 4 and a second raw material phase 4; wherein, The amount ratio of the first raw material phase 4 to the raw material phase 3 is (1-2): (1-2); and / or, The usage ratio of the first raw material phase four to the second raw material phase four is (1~2):(1~2).
3. The method for swelling seed microspheres according to claim 2, characterized in that: The mass percentages of styrene, divinylbenzene, porogen, emulsifier and initiator in the first raw material phase 4 are (1.5-3): (1-4): (1-2): (0.5-1.5): (0.5-1.5); and / or, The mass percentages of styrene, divinylbenzene, emulsifier and initiator in the second raw material phase four are (1.5~3):(1~4):(0.5~1.5):(0.5~1.5).
4. The method for swelling seed microspheres according to any one of claims 1 to 3, characterized in that: Calculated according to the mass of the first raw material phase 4, the mass ratio of the first raw material phase 4 of each added batch to the total mass of the first raw material phase 4 is 20-50wt%; and / or, Calculated according to the mass of the second raw material phase four, the mass ratio of the amount of the second raw material phase four in each added batch to the total amount of the second raw material phase four is 20-50wt%.
5. The method for swelling seed microspheres according to claim 4, characterized in that: The seed microspheres have a polydispersity coefficient of 1-1.2 and a particle size of 0.2-4 μm.
6. The method for swelling seed microspheres according to claim 4, characterized in that: The seed microspheres have a polydispersity coefficient of 1.02-1.1 and a particle size of 0.5-3.5 μm.
7. A resin microsphere particle or a group of resin microsphere particles, characterized in that: The resin microsphere particles are prepared by the method according to any one of claims 1 to 6.
8. A resin microsphere particle or a group of resin microsphere particles prepared by the method according to any one of claims 1 to 6, characterized in that: The particle size of the resin microsphere particles is 4-9 μm; and / or, The crosslinking degree of the resin microsphere particles is 30% - 45%; and / or, The polydispersity coefficient of the resin microsphere particles contained in the resin microsphere particle group is 1 to 1.
2.
9. A chromatographic packing, characterized in that: The chromatographic filler comprises the resin microsphere particles prepared by the method of any one of claims 1 to 6; and / or the resin microsphere particle group of any one of claims 7 to 8.