A kind of adhesive and preparation method thereof

Through the combination of modified water-based polyurethane dispersion and dialdehyde starch-modified isocyanate end-capping curing agent, combined with other additives, the problems of slow film-forming speed, low initial tack and poor water resistance of water-based polyurethane adhesives are solved, achieving high Adhesive and waterproof properties, adhesive preparation that meets environmental requirements.

CN118374258BActive Publication Date: 2024-10-29SHANGHAI JINGQIU NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410831340.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Existing water-based polyurethane adhesives have problems such as slow film formation speed, low initial adhesion, poor water resistance and solvent resistance, low hardness and poor hand feel. It is difficult to meet the needs of high adhesion and waterproofness. At the same time, Does not meet environmental protection requirements.

Method used

Using modified water-based polyurethane dispersion and dialdehyde starch modified isocyanate end-capping curing agent, combined with defoaming agent, thickener, silane coupling agent, mussel mucin and filler, through ball milling and ultrasonic dispersion technology, a product with Adhesive with excellent adhesion and water resistance.

Benefits of technology

It significantly improves the adhesiveness, waterproofness and environmental protection performance of the adhesive, meets the requirements of high adhesiveness and green environmental protection, and maintains good adhesion effect in humid environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to an adhesive and a preparation method thereof, and belongs to the technical field of waterborne polyurethane adhesives. The adhesive is composed of three components A, B, and C in a mass ratio of 10: (1-1.5): (5-6), and in terms of mass fractions: component A includes: 50-75 parts of a modified waterborne polyurethane dispersion and 30-40 parts of deionized water; component B includes: 50-70 parts of a dialdehyde starch-modified isocyanate-terminated curing agent; component C includes: 5-7 parts of a defoamer, 2-4 parts of a thickener, 1-2 parts of a silane coupling agent, 3-5 parts of mussel mucin, 25-35 parts of a filler, and 1-2 parts of an auxiliary agent. In the present invention, avocado fat-modified nano-montmorillonite and an aqueous polyurethane prepared by reacting sucrose and sorbitol with a hydrophilic monomer are mixed to obtain a modified waterborne polyurethane dispersion, which is cured by a dialdehyde starch-modified isocyanate curing agent. Under the joint action of other auxiliary agents, the prepared adhesive has high adhesion and waterproofness, and conforms to the concept of green environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waterborne polyurethane adhesives and relates to an adhesive and a preparation method thereof. Background Art

[0002] Adhesives are organic or inorganic, natural or synthetic substances that can connect the same, two or more homogeneous or heterogeneous parts (or materials) together and have sufficient strength after curing. They are generally divided into natural polymer compounds, synthetic polymer compounds or inorganic compounds. With the deepening of the current environmental protection concept, many industrial production fields are gradually replacing solvent-based adhesives with water-based adhesives. Among them, the more prominent material used is water-based polyurethane adhesive. Water-based polyurethane adhesive has strong comprehensive performance and flexible formula design. It can be appropriately adjusted according to actual use needs. It is currently widely used in many fields and has a good improvement effect on the performance of polyurethane adhesives.

[0003] Polyurethane adhesive is an important adhesive widely used in many fields. Its main resin contains a large number of active reactive groups and polar groups, which can bond a variety of substrates. At present, water-based polyurethane adhesive uses water as the dispersion medium, and has the advantages of no pollution, no toxicity, good compatibility, excellent mechanical properties and easy modification. However, water-based polyurethane adhesive also has some disadvantages, such as slow film formation speed, low initial adhesion, poor water resistance and solvent resistance, low hardness and poor feel.

[0004] Therefore, it is necessary to design and develop a water-based polyurethane adhesive with high adhesion, waterproofness and environmental protection requirements. Summary of the invention

[0005] The object of the present invention is to provide an adhesive and a preparation method thereof, which have excellent adhesion and waterproof properties and are green and environmentally friendly.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] An adhesive, comprising component A, component B and component C, wherein, by mass:

[0008] The component A comprises: 50-75 parts of modified waterborne polyurethane dispersion and 30-40 parts of deionized water;

[0009] The B component includes: 50-70 parts of dialdehyde starch modified isocyanate terminated curing agent;

[0010] The C component includes: 5-7 parts of defoamer, 2-4 parts of thickener, 1-2 parts of silane coupling agent, 3-5 parts of mussel mucin, 25-35 parts of filler, and 1-2 parts of auxiliary agent;

[0011] The preparation process of the modified waterborne polyurethane dispersion is as follows:

[0012] 3-5 parts of avocado fat and 20-35 parts of nano-montmorillonite were ground by a ball mill at a speed of 400 r / min for 3 hours to obtain avocado fat-modified nano-montmorillonite;

[0013] Under nitrogen conditions, 30 parts of sucrose and 30 parts of sorbitol are mixed evenly, and then 0.5-1 parts of sodium hydroxide are added, and the mixture is reacted at 90-94° C. for 3-4 hours to obtain a polyether polyol; 60-80 parts of polyether polyol and 15-30 parts of isocyanate crosslinking agent are added to a reactor, and the mixture is stirred and heated to 75-90° C. for reaction for 4 hours to obtain a polyurethane prepolymer having an NCO end group, and then 1-2.5 parts of a chain extender are added for reaction, and then 3-7 parts of a hydrophilic monomer are added, and the reaction is continued by stirring for 7-8 hours, and then 5-8 parts of avocado fat-modified nano-montmorillonite are added and mixed evenly to obtain a modified waterborne polyurethane dispersion, wherein the isocyanate crosslinking agent is 1,3-diisobenzocyanate.

[0014] As a preferred technical solution of the present invention, the defoaming agent is one of BYK-011, BYK-035 and BYK-037.

[0015] As a preferred technical solution of the present invention, the thickener is one of hydroxyethyl cellulose, guar gum and xanthan gum.

[0016] As a preferred technical solution of the present invention, the silane coupling agent is one of KH550 and KH560.

[0017] As a preferred technical solution of the present invention, the filler is one or more of calcium carbonate, talcum powder, silicon powder, aluminum hydroxide, and calcium sulfate whiskers.

[0018] As a preferred technical solution of the present invention, the chain extender is one of dimethylolpropionic acid, hexamethylenediamine and dimethylolbutyric acid.

[0019] As a preferred technical solution of the present invention, the hydrophilic monomer is one of 1,4-butanediol and neopentyl glycol.

[0020] As a preferred technical solution of the present invention, the auxiliary agent is one of 2,4,6-tris(dimethylaminomethyl)phenol and N,N-dimethylbenzylamine.

[0021] As a preferred technical solution of the present invention, the modified isocyanate-terminated curing agent is modified by dialdehyde starch, and the specific preparation process is as follows:

[0022] 30-35 parts of dialdehyde starch and 20-23 parts of hexamethylene diisocyanate were reacted in ethyl acetate at 80° C. for 6 hours to obtain a dialdehyde starch modified isocyanate-terminated curing agent.

[0023] A method for preparing an adhesive, the preparation process is as follows:

[0024] Under nitrogen protection, component A and component B are ultrasonically dispersed for 2-3 hours at a temperature of 70-80°C. After uniform dispersion, component C is added and stirred to obtain the adhesive, wherein the mass ratio of component A, component B and component C is 10:(1-1.5):(5-6).

[0025] Avocado butter contains long-chain fatty acid structures and has good wettability. Nano-montmorillonite has a huge specific surface area and porous structure. The fatty acids and other active ingredients in avocado butter will react with the surface of nano-montmorillonite to form stable substances. Ball milling can make avocado butter more evenly dispersed, and the long-chain structure can enter the lamellar structure of nano-montmorillonite, so that nano-montmorillonite also has good wettability.

[0026] When preparing modified waterborne polyurethane dispersions, sucrose and sorbitol are used as raw materials. Sucrose, as a polyhydroxy compound, has excellent biodegradability, which contributes to the environmental friendliness of polyurethane products. Through the modification of sucrose, the water resistance and thermal stability of polyurethane materials have been significantly improved. The molecular structure characteristics of sucrose enable it to form multiple crosslinking points, and then synthesize waterborne polyurethane with a network structure under catalyst-free conditions. Sorbitol can be used as a chain extender, contains a polyhydroxy structure, and is easy to generate sorbitol polyether, which can react with isocyanate in the polymerization reaction to form hydrogen bonds, thereby reducing the surface tension of polyurethane and significantly improving the stability and strength of polyurethane. The multiple oxidized hanging chains and hydroxyl reactive polymer characteristics in sorbitol polyether enable it to control the water content of the reactant and undergo a ring-opening attack reaction with the hydrophilic group of isocyanate to form a delicate arrangement structure.

[0027] Sucrose and sorbitol are both biodegradable, which helps reduce the environmental impact of polyurethane products.

[0028] By adding modified nano-montmorillonite during the preparation process of modified waterborne polyurethane, the modified nano-montmorillonite can be used to improve the wettability of waterborne polyurethane. Since it has been treated with avocado butter, the surface tension in the solution is reduced, the nano-montmorillonite is easier to disperse in the waterborne polyurethane, and it can help to improve the adhesion and coverage between the nano-montmorillonite and the waterborne polyurethane.

[0029] Isocyanate contains compounds with isocyanate groups (-NCO), which are very active and easily react with compounds containing active hydrogen. Dialdehyde starch is a product obtained by oxidation of starch. Its molecules contain multiple aldehyde groups, which can react with isocyanate groups. Under appropriate reaction temperature and stirring conditions, hexamethylene diisocyanate and dialdehyde starch are evenly mixed, and the isocyanate group (-NCO) reacts with the aldehyde group (-CHO) in dialdehyde starch to form urea bonds and urethane bonds. The formation of these chemical bonds forms a cross-linked network structure between starch molecules, thereby improving the water resistance and adhesive strength of the curing agent. The water resistance and adhesive strength of the curing agent can be significantly improved by modifying isocyanate with dialdehyde starch, because the network structure formed by the cross-linking reaction can effectively prevent the penetration of water molecules and enhance the interaction between molecules. The modified curing agent also has good wet adhesion properties and can maintain good adhesion in a humid environment.

[0030] At the same time, the addition of mussel mucin improves the cohesiveness and water resistance of the adhesive, thereby improving its adhesion and tensile strength. Mussel mucin contains a high proportion of lysine and dopa groups (i.e., DOPA). The DOPA group can participate in chemical reactions and cross-link with other groups (such as hydroxyl and carboxyl) in the water-based polyurethane adhesive, thereby enhancing the intermolecular forces of the adhesive. This cross-linking can improve the water resistance and cohesiveness of the adhesive, making it less likely to be washed away or decomposed in water. Mussel mucin itself has strong water resistance, and its addition can improve the stability of water-based polyurethane adhesives in humid environments.

[0031] Beneficial effects of the present invention:

[0032] In the present invention, nano-montmorillonite is modified by using avocado fat, and mixed with an aqueous polyurethane prepared by reacting sucrose and sorbitol with a hydrophilic monomer to obtain a modified aqueous polyurethane dispersion, which is then cured by an isocyanate curing agent modified with dialdehyde starch. Under the combined action of other additives, the prepared adhesive has high adhesion and waterproof properties and complies with the concept of green environmental protection. DETAILED DESCRIPTION

[0033] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0034] Raw materials used in the following examples and comparative examples:

[0035] The isocyanate crosslinking agent was 1,3-diisophenylcyanate: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., product number: P160603;

[0036] Ordinary polyether polyol: polypropylene glycol, purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: P815574;

[0037] Avocado butter: purchased from Tesco Chemical (Hubei) Co., Ltd., model: 25kg / barrel;

[0038] Nano-montmorillonite: purchased from Zhejiang Fenghong New Materials Co., Ltd., brand: Walter;

[0039] Sucrose: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., product number: S112224;

[0040] Sorbitol: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: D796624;

[0041] Dimethylolpropionic acid: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: B802228;

[0042] 1,4-Butanediol: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., product number: B11039;

[0043] BYK-011: purchased from Guangzhou Baohua Trading Co., Ltd.;

[0044] BYK-035: purchased from Guangzhou Baohua Trading Co., Ltd.;

[0045] Hydroxyethyl cellulose: purchased from Shanghai Yuanye Biotechnology Co., Ltd., product number: S14167-250g;

[0046] KH550: purchased from Shanghai Yuanye Biotechnology Co., Ltd., product number: S15028-500ml;

[0047] KH560: purchased from Shanghai Yuanye Biotechnology Co., Ltd., product number: S15029-500ml;

[0048] Hexamethylenediamine: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., product number: H103909;

[0049] Mussel mucin: purchased from Xi'an Zebang Biotechnology Co., Ltd.;

[0050] Calcium carbonate: purchased from Shanghai Haohong Biopharmaceutical Technology Co., Ltd., product number: 1440000;

[0051] 2,4,6-Tris(dimethylaminomethyl)phenol: purchased from Wuhan Penglei Biotechnology Co., Ltd.;

[0052] Dialdehyde starch: purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd., product number: PA97285;

[0053] Hexamethylene diisocyanate: purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., product number: H106723;

[0054] Dimethylolpropionic acid: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: B802228;

[0055] Neopentyl glycol: purchased from Shanghai MacLean Biochemical Technology Co., Ltd., product number: N821327.

[0056] Example 1

[0057] Component A includes: 50 parts of modified waterborne polyurethane dispersion and 30 parts of deionized water;

[0058] Component B includes: 50 parts of dialdehyde starch modified isocyanate terminated curing agent;

[0059] Component C includes: 5 parts BYK-011, 2 parts hydroxyethyl cellulose, 1 part KH550, 3 parts mussel mucin, 25 parts calcium carbonate, 1 part 2,4,6-tris(dimethylaminomethyl)phenol;

[0060] Preparation of modified waterborne polyurethane dispersion:

[0061] 3 parts of avocado fat and 20 parts of nano-montmorillonite were ground by a ball mill at a speed of 400 r / min for 3 hours to obtain avocado fat-modified nano-montmorillonite;

[0062] Under nitrogen conditions, 30 parts of sucrose and 30 parts of sorbitol were mixed evenly, and then 0.5 parts of sodium hydroxide were added, and the mixture was reacted at 90°C for 4 hours to obtain polyether polyol; 60 parts of polyether polyol and 15 parts of isocyanate crosslinking agent were added to a reactor, and the mixture was stirred and heated to 75°C for reaction for 4 hours to obtain a polyurethane prepolymer with an NCO end group, and then 1 part of dihydroxymethylpropionic acid was added for reaction, followed by 3 parts of 1,4-butanediol, and the reaction was continued with stirring for 7 hours, and then 5 parts of avocado fat-modified nano-montmorillonite were added and mixed evenly to obtain a modified waterborne polyurethane dispersion.

[0063] The modified isocyanate-terminated curing agent is modified by dialdehyde starch, and the specific preparation process is as follows:

[0064] 30 parts of dialdehyde starch and 20 parts of hexamethylene diisocyanate were reacted in ethyl acetate at 80° C. for 6 hours to obtain a dialdehyde starch modified isocyanate-terminated curing agent.

[0065] Prepare the adhesive:

[0066] Under nitrogen protection, component A and component B were ultrasonically dispersed for 2 hours at a temperature of 70°C. After uniform dispersion, component C was added and stirred to obtain an adhesive, wherein the mass ratio of component A, component B and component C was 10:1:5.

[0067] Example 2

[0068] Component A includes: 65 parts of modified waterborne polyurethane dispersion and 36 parts of deionized water;

[0069] Component B includes: 54 parts of dialdehyde starch modified isocyanate terminated curing agent;

[0070] Component C includes: 6 parts BYK-035, 3 parts hydroxyethyl cellulose, 1.5 parts KH550, 4 parts mussel mucin, 30 parts calcium carbonate, 1.5 parts 2,4,6-tris(dimethylaminomethyl)phenol;

[0071] Preparation of modified waterborne polyurethane dispersion:

[0072] 4 parts of avocado fat and 28 parts of nano-montmorillonite were ground by a ball mill at a speed of 400 r / min for 3 h to obtain avocado fat-modified nano-montmorillonite;

[0073] Under nitrogen conditions, 30 parts of sucrose and 30 parts of sorbitol were mixed evenly, and then 0.8 parts of sodium hydroxide was added, and the mixture was reacted at 93°C for 3.5 hours to obtain polyether polyol; 71 parts of polyether polyol and 22 parts of isocyanate crosslinking agent were added to a reactor, and the mixture was stirred and heated to 82°C for reaction for 4 hours to obtain a polyurethane prepolymer with an NCO end group, and then 2 parts of hexamethylenediamine were added for reaction, followed by 5 parts of 1,4-butanediol, and the reaction was continued with stirring for 7.5 hours, and then 7 parts of avocado fat-modified nano-montmorillonite were added and mixed evenly to obtain a modified waterborne polyurethane dispersion.

[0074] The modified isocyanate-terminated curing agent is modified by dialdehyde starch, and the specific preparation process is as follows:

[0075] 33 parts of dialdehyde starch and 21 parts of hexamethylene diisocyanate were reacted in ethyl acetate at 80° C. for 6 hours to obtain a dialdehyde starch modified isocyanate-terminated curing agent.

[0076] Prepare the adhesive:

[0077] Under nitrogen protection, component A and component B were ultrasonically dispersed for 2.5 hours at a temperature of 75°C. After uniform dispersion, component C was added and stirred to obtain an adhesive, wherein the mass ratio of component A, component B and component C was 10:1.2:5.5.

[0078] Example 3

[0079] Component A includes: 75 parts of modified waterborne polyurethane dispersion and 40 parts of deionized water;

[0080] Component B includes: 70 parts of dialdehyde starch modified isocyanate terminated curing agent;

[0081] Component C includes: 7 parts BYK-011, 4 parts hydroxyethyl cellulose, 2 parts KH560, 5 parts mussel mucin, 35 parts calcium carbonate, 2 parts 2,4,6-tris(dimethylaminomethyl)phenol;

[0082] Preparation of modified waterborne polyurethane dispersion:

[0083] Grind 5 parts of avocado fat and 35 parts of nano-montmorillonite in a ball mill at a speed of 400 r / min for 3 h to obtain avocado fat-modified nano-montmorillonite;

[0084] Under nitrogen conditions, 30 parts of sucrose and 30 parts of sorbitol were mixed evenly, and 1 part of sodium hydroxide was added, and the mixture was reacted at 94°C for 3 hours to obtain polyether polyol; 80 parts of polyether polyol and 30 parts of isocyanate crosslinking agent were added to a reactor, and the mixture was heated to 90°C with stirring and reacted for 4 hours to obtain a polyurethane prepolymer having an NCO end group, and 2.5 parts of dihydroxymethylpropionic acid were added to react, followed by adding 7 parts of neopentyl glycol, and the mixture was stirred and reacted for 8 hours, and then 8 parts of avocado fat-modified nano-montmorillonite were added and mixed evenly to obtain a modified waterborne polyurethane dispersion.

[0085] The modified isocyanate-terminated curing agent is modified by dialdehyde starch, and the specific preparation process is as follows:

[0086] 35 parts of dialdehyde starch and 23 parts of hexamethylene diisocyanate were reacted in ethyl acetate at 80° C. for 6 hours to obtain a dialdehyde starch modified isocyanate-terminated curing agent.

[0087] Prepare the adhesive:

[0088] Under nitrogen protection, component A and component B were ultrasonically dispersed for 3 hours at 80°C. After uniform dispersion, component C was added and stirred to obtain an adhesive, wherein the mass ratio of component A, component B and component C was 10:1.5:6.

[0089] Comparative Example 1

[0090] The difference between Comparative Example 1 and Example 2 is that the nano-montmorillonite in Comparative Example 1 is not modified by avocado fat, and the other operations are the same.

[0091] Comparative Example 2

[0092] The difference between Comparative Example 2 and Example 2 is that in Comparative Example 2, no modified nano-montmorillonite is added when preparing the modified aqueous polyurethane dispersion, and the other operations are the same.

[0093] Comparative Example 3

[0094] The difference between Comparative Example 3 and Example 2 is that in Comparative Example 3, the isocyanate curing agent is not modified by dialdehyde starch, and the other operations are the same.

[0095] Comparative Example 4

[0096] The difference between Comparative Example 4 and Example 2 is that mussel mucin is not added in Comparative Example 4, and the other operations are the same.

[0097] Comparative Example 5

[0098] The difference between Comparative Example 5 and Example 2 is that the raw material of the waterborne polyurethane used in Comparative Example 5 is common polyether polyol, and the other operations are the same.

[0099] Performance Test:

[0100] 1. The adhesives prepared in the examples and comparative examples were cured at 100° C. for 8 h;

[0101] Weigh a certain mass of the solidified material and soak it in water for 48 hours. Take it out and wipe off the surface moisture, weigh it, and calculate the water absorption rate W, W=(mM) / Mⅹ100%, M is the initial mass, and m is the mass after water absorption.

[0102] 2. Refer to JC / T 863-2011 "Polymer Waterproof Membrane Adhesive" to test the viscosity, non-volatile content, application period, and adhesion under shear state;

[0103] The results are as follows:

[0104]

[0105] According to the above data, the data in the examples are better than those in the comparative examples. The waterborne polyurethane prepared by the modification method used in the present invention has a lower water absorption rate and thus has high water resistance and waterproofness.

[0106] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. An adhesive, comprising component A, component B and component C, It is characterized in that In parts by mass: The component A comprises: 50-75 parts of modified waterborne polyurethane dispersion and 30-40 parts of deionized water; The B component includes: 50-70 parts of dialdehyde starch modified isocyanate terminated curing agent; The C component includes: 5-7 parts of defoamer, 2-4 parts of thickener, 1-2 parts of silane coupling agent, 3-5 parts of mussel mucin, 25-35 parts of filler, and 1-2 parts of auxiliary agent; The preparation process of the modified waterborne polyurethane dispersion is as follows: 3-5 parts of avocado fat and 20-35 parts of nano-montmorillonite were ground by a ball mill at a speed of 400 r / min for 3 hours to obtain avocado fat-modified nano-montmorillonite; Under nitrogen conditions, 30 parts of sucrose and 30 parts of sorbitol are mixed evenly, and then 0.5-1 parts of sodium hydroxide are added, and the mixture is reacted at 90-94° C. for 3-4 hours to obtain a polyether polyol; 60-80 parts of polyether polyol and 15-30 parts of isocyanate crosslinking agent are added to a reactor, and the mixture is stirred and heated to 75-90° C. for reaction for 4 hours to obtain a polyurethane prepolymer having an NCO end group, and then 1-2.5 parts of a chain extender are added for reaction, and then 3-7 parts of a hydrophilic monomer are added, and the reaction is continued by stirring for 7-8 hours, and then 5-8 parts of avocado fat-modified nano-montmorillonite are added and mixed evenly to obtain a modified waterborne polyurethane dispersion, wherein the isocyanate crosslinking agent is 1,3-diisobenzocyanate.

2. The adhesive according to claim 1, Features: The defoamer is one of BYK-011, BYK-035 and BYK-037.

3. The adhesive according to claim 1, Features: The thickener is one of hydroxyethyl cellulose, guar gum and xanthan gum.

4. The adhesive according to claim 1, Features: The silane coupling agent is one of KH550 and KH560.

5. The adhesive according to claim 1, Features: The filler is one or more of calcium carbonate, talcum powder, silicon powder, aluminum hydroxide, and calcium sulfate whisker.

6. The adhesive according to claim 1, Features: The chain extender is one of dimethylol propionic acid, hexamethylenediamine and dimethylol butyric acid.

7. The adhesive according to claim 1, Features: The hydrophilic monomer is one of 1,4-butanediol and neopentyl glycol.

8. The adhesive according to claim 1, Features: The auxiliary agent is one of 2,4,6-tris(dimethylaminomethyl)phenol and N,N-dimethylbenzylamine.

9. The adhesive according to claim 1, Features: The modified isocyanate-terminated curing agent is modified by dialdehyde starch, and the specific preparation process is as follows: 30-35 parts of dialdehyde starch and 20-23 parts of hexamethylene diisocyanate were reacted in ethyl acetate at 80° C. for 6 hours to obtain a dialdehyde starch modified isocyanate-terminated curing agent.

10. A method for preparing the adhesive according to any one of claims 1 to 9, It is characterized in that The preparation process is as follows: Under nitrogen protection, component A and component B are ultrasonically dispersed for 2-3 hours at a temperature of 70-80°C. After uniform dispersion, component C is added and stirred to obtain the adhesive, wherein the mass ratio of component A, component B and component C is 10:(1-1.5):(5-6).

Citation Information

Patent Citations

  • Starch-containing thermoplastic or elastomer compositions, and method for preparing such compositions

    AU2009259118A1

  • Nonformaldehyde nonpoisonous adhesive and preparation method thereof

    CN101709211A