A flexible deep ultraviolet photosynaptic transistor and its preparation method and application
By adopting a flexible structure and specific active layer design in the deep ultraviolet photoelectric synaptic transistor, the problem of slow response speed is solved, fast response and high signal-to-noise ratio are achieved, and it is suitable for large-scale applications in the field of neuromorphic computing.
Patent Information
- Application Number
- CN202410483344.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-04-22
Smart Images

Figure CN118380501B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of neuromorphic computing technology, and in particular to a flexible deep ultraviolet photosynaptic transistor and a preparation method and application thereof. Background Art
[0002] The von Neumann architecture is a memory structure that combines program instruction memory and data memory. It is the basic computer architecture for solving complex and structured mathematical problems. However, due to the physical separation of storage modules and processors, this traditional architecture faces bottlenecks of high energy consumption and low efficiency when dealing with complex computing and cognitive tasks. In contrast, the neuromorphic computing architecture is inspired by the human brain and can imitate the functions of the human brain. It can achieve high-performance data processing and storage parallel operations, and is particularly suitable for solving complex unstructured problems based on past experience and memory. Synapses are an important part of the human brain and a key structure for learning and memory. Therefore, the preparation of devices with synaptic functions is the basis for realizing neuromorphic computing. More than 70% of the information that humans perceive from the outside world comes from vision. The sensory neurons of the retina in the human visual system can not only respond to light stimuli, but also temporarily memorize and process visual information. Therefore, neuromorphic optoelectronic synapses are extremely attractive in simulating human vision.
[0003] Deep ultraviolet photosynaptic transistors can detect deep ultraviolet light and have broad application prospects in the fields of optical communications, imaging, military surveillance, target detection and capture, and missile launch detection. Deep ultraviolet photosynaptic transistors usually use wide-bandgap semiconductors (such as indium gallium zinc oxygen, zinc oxide, vanadium oxide, gallium oxide, etc.), which have high deep ultraviolet light responsivity and extremely long-lasting photoconductivity, providing feasibility for simulating synaptic characteristics. However, the existing photosynaptic transistors made of metal oxide semiconductors have limited charge carrier mobility, resulting in slow response speed and inability to effectively respond to short-duration weak light pulses, thereby limiting the overall decision-making speed of neuromorphic computing systems.
[0004] Therefore, it is of great significance to develop a deep ultraviolet photosynaptic transistor with fast response capability. Summary of the invention
[0005] The object of the present invention is to provide a flexible deep ultraviolet photoelectric synaptic transistor and a preparation method and application thereof.
[0006] The technical solution adopted by the present invention is:
[0007] A flexible deep ultraviolet photoelectric synaptic transistor comprises a flexible substrate, a gate dielectric layer, an active layer, a source-drain electrode layer, a hydrophobic barrier layer and a near-ultraviolet light barrier layer which are stacked in sequence, and also comprises a gate electrode which is arranged inside the gate dielectric layer and contacts the flexible substrate; the active layer comprises a first indium tin magnesium oxide layer, an indium tin zinc oxide layer and a second indium tin magnesium oxide layer which are stacked in sequence.
[0008] Preferably, the thickness of the first indium tin magnesium oxide layer is 5 nm to 30 nm.
[0009] Preferably, the thickness of the indium tin zinc oxide layer is 10 nm to 40 nm.
[0010] Preferably, the second indium tin magnesium oxide layer has a thickness of 5 nm to 30 nm.
[0011] Preferably, the flexible substrate is one of a flexible polyimide (PI) substrate, a flexible polyethylene terephthalate (PET) substrate, and a flexible polyether substrate.
[0012] Preferably, the gate dielectric layer is composed of one of neodymium aluminum oxide, aluminum oxide, silicon dioxide and zirconium oxide.
[0013] Preferably, the gate dielectric layer has a thickness of 100 nm to 300 nm.
[0014] Preferably, the gate electrode is composed of at least one of Al and Nd.
[0015] Preferably, the gate electrode has a thickness of 80 nm to 120 nm.
[0016] Preferably, the source electrode in the source-drain electrode layer is one of an ITO electrode, an Al electrode, a Cu electrode and an Au electrode.
[0017] Preferably, the drain electrode in the source-drain electrode layer is one of an ITO electrode, an Al electrode, a Cu electrode and an Au electrode.
[0018] Preferably, the hydrophobic barrier layer is composed of at least one of n-octyltriethoxysilane, octadecyltrimethoxysilane and octadecyltrichlorosilane.
[0019] Preferably, the thickness of the hydrophobic barrier layer is 2 nm to 10 nm.
[0020] Preferably, the near-ultraviolet light blocking layer is composed of an optically transparent silicone resin and a near-ultraviolet light absorber.
[0021] Preferably, the mass ratio of the optically transparent silicone resin to the near-ultraviolet light absorber is 1:0.05-0.25.
[0022] Preferably, the optically transparent silicone resin is at least one of TSE399-C produced by Momentive and LUMISILLR7600 produced by Wacker Chemicals.
[0023] Preferably, the near-ultraviolet light absorber is diethylaminohydroxybenzoyl hexyl benzoate.
[0024] Further preferably, the near-ultraviolet light absorber is the ultraviolet light absorber DHHB (the main component of which is diethylaminohydroxybenzoyl hexyl benzoate).
[0025] Preferably, the thickness of the near-ultraviolet light blocking layer is 100 nm to 600 nm.
[0026] A method for preparing the flexible deep ultraviolet photosynaptic transistor as described above comprises the following steps:
[0027] 1) depositing a gate electrode and a gate dielectric layer in sequence on a single side of a flexible substrate;
[0028] 2) depositing an indium tin magnesium oxide layer, an indium tin zinc oxide layer and an indium tin magnesium oxide layer on the surface of the gate dielectric layer in sequence to form an active layer;
[0029] 3) depositing a source electrode and a drain electrode on the surface of the active layer to form a source-drain electrode layer;
[0030] 4) placing the device obtained in step 3) in an atmosphere containing a hydrophobic substance to form a hydrophobic barrier layer;
[0031] 5) Covering the surface of the hydrophobic barrier layer with a near-ultraviolet light blocking material to form a near-ultraviolet light blocking layer, thereby obtaining a flexible deep ultraviolet photosynaptic transistor.
[0032] An array substrate comprises the above-mentioned flexible deep ultraviolet photoelectric synapse transistor.
[0033] A neuromorphic computer comprises the flexible deep ultraviolet photosynaptic transistor.
[0034] The beneficial effects of the present invention are as follows: the flexible deep ultraviolet photosynaptic transistor of the present invention has the advantages of fast response speed, good flexibility, stable performance, etc. It can improve the overall decision-making speed of the neuromorphic computing system and is suitable for large-scale application in the field of neuromorphic computing.
[0035] Specifically:
[0036] 1) The flexible deep ultraviolet photosynaptic transistor of the present invention adopts a sandwich-structured oxide semiconductor active layer, which includes two oxide semiconductor layers with different bandgap widths and different work functions, so that the generated photoelectrons can be quickly transmitted to the collector under the action of the vertical gate electric field. This design utilizes the conduction band offset effect, so that the photoelectrons are not affected by the scattering of the positive center during the transfer from the indium tin zinc oxide layer to the indium tin magnesium oxide layer, thereby realizing the transmission of fast and large currents, and thus being able to achieve fast response, especially under high-frequency illumination conditions. In addition, by utilizing the continuous photoconductivity phenomenon unique to oxide semiconductors and the carrier capture effect introduced at the interface between the indium tin zinc oxide layer and the indium tin magnesium oxide layer, a variety of synaptic plasticities can be simulated under conditions of shorter illumination time or weaker illumination intensity; finally, because the active layer has a higher film quality and a suitable oxygen vacancy concentration, the flexible deep ultraviolet photosynaptic transistor has excellent electrical properties that are difficult for other flexible deep ultraviolet photosynaptic transistors to have, and has a broader application prospect;
[0037] 2) The flexible deep ultraviolet photosynaptic transistor of the present invention is provided with a near ultraviolet light blocking layer, which can effectively reduce the interference of near ultraviolet light in the environment on the deep ultraviolet photosynaptic transistor, thereby improving the signal-to-noise ratio of the neuromorphic computing system and making the performance of the system more stable and reliable;
[0038] 3) The present invention utilizes the persistent photoconductivity phenomenon unique to oxide semiconductors to enable the flexible deep ultraviolet photosynaptic transistor to have photoelectric memory characteristics, and can simulate a variety of synaptic plasticity, making the flexible deep ultraviolet photosynaptic transistor more flexible in neuromorphic computing systems;
[0039] 4) The flexible deep ultraviolet photosynaptic transistor of the present invention adopts a flexible substrate, so that the flexible deep ultraviolet photosynaptic transistor can be flexibly applied to various irregular surfaces, thereby broadening its scope of application in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is a schematic structural diagram of the flexible deep ultraviolet photosynaptic transistor of the present invention.
[0041] Description of the accompanying drawings: 10, flexible substrate; 20, gate electrode; 30, gate dielectric layer; 40, active layer; 401, first indium tin magnesium oxide layer; 402, indium tin zinc oxide layer; 403, second indium tin magnesium oxide layer; 50, source-drain electrode layer; 501, source electrode; 502, drain electrode; 60, hydrophobic barrier layer; 70, near-ultraviolet light blocking layer.
[0042] Figure 2 2 is a transfer characteristic curve of the flexible deep ultraviolet photosynaptic transistor of the embodiment.
[0043] Figure 3 This is the transfer characteristic curve of the flexible deep ultraviolet photosynaptic transistor of comparative example 1.
[0044] Figure 4 1 is an output characteristic curve of the flexible deep ultraviolet photosynaptic transistor of an embodiment.
[0045] Figure 5 This is the output characteristic curve of the flexible deep ultraviolet photosynaptic transistor of comparative example 1.
[0046] Figure 6 This is a diagram showing changes in postsynaptic current of the flexible deep ultraviolet photosynaptic transistor of the embodiment in response to a deep ultraviolet double pulse signal with a wavelength of 254 nm.
[0047] Figure 7 This is a graph showing the change in postsynaptic current of the flexible deep ultraviolet photosynaptic transistor of comparative example 1 in response to a deep ultraviolet double pulse signal with a wavelength of 254 nm. DETAILED DESCRIPTION
[0048] The present invention will be further explained and illustrated below in conjunction with specific embodiments.
[0049] Example:
[0050] A flexible deep ultraviolet photosynaptic transistor (schematic diagram as shown in FIG. Figure 1 ), which is composed of a flexible substrate 10, a gate electrode 20, a gate dielectric layer 30, an active layer 40, a source-drain electrode layer 50, a hydrophobic barrier layer 60 and a near-ultraviolet light blocking layer 70; the flexible substrate 10, the gate dielectric layer 30, the active layer 40, the source-drain electrode layer 50, the hydrophobic barrier layer 60 and the near-ultraviolet light blocking layer 70 are stacked in sequence from bottom to top; the active layer 40 is formed by stacking a first indium tin magnesium oxide layer 401, an indium tin zinc oxide layer 402 and a second indium tin magnesium oxide layer 403 in sequence from bottom to top; the source-drain electrode layer 50 includes a source electrode 501 and a drain electrode 502; the gate electrode 20 is arranged inside the gate dielectric layer 30 and contacts with the flexible substrate 10.
[0051] The preparation method of the above-mentioned flexible deep ultraviolet photosynaptic transistor is as follows:
[0052] 1) A 100 nm thick Al-Nd alloy film is deposited on a single side of a 18 μm thick polyimide substrate (the back side is first bonded to a glass substrate as a support through a pressure sensitive adhesive, and the glass substrate is removed after the entire preparation process is completed) by direct current magnetron sputtering, and a gate electrode is formed by patterning through photolithography. The polyimide substrate with the prepared gate electrode is used as an anode and a stainless steel plate is used as a cathode. The polyimide substrate is placed in an ethylene glycol solution with a mass fraction of 4% ammonium tartrate. A constant current is first applied between the anode and the cathode. When the voltage between the anode and the cathode increases linearly with time to 100 V, the voltage is kept constant until the current density between the anode and the cathode decreases to 0.001 mA / cm 2 , forming an aluminum-neodymium oxide layer with a thickness of 200 nm, and then patterning the aluminum-neodymium oxide layer to form a gate dielectric layer;
[0053] 2) The polyimide substrate prepared with the gate dielectric layer is placed in a patterned metal mask and fixed, and a 10 nm thick indium tin magnesium oxide film, a 20 nm thick indium tin zinc oxide film and a 10 nm thick indium tin magnesium oxide film are sequentially deposited as the oxide active layer of the sandwich structure by continuous multi-target co-sputtering, and then placed on a hot stage for annealing at an air atmosphere and a temperature of 350°C for 3 hours; the process parameters of the continuous multi-target co-sputtering are as follows: the chamber pressure is set to 0.5 Pa during sputtering, and the gas used is The atmosphere was oxygen and argon, and the flow rates were set to 6 sccm and 10 sccm respectively. The sputtering temperature was set to 300°C. The targets used for sputtering the indium tin magnesium oxide film were polycrystalline indium tin oxide and polycrystalline magnesium oxide. The sputtering time was 30 s. The targets used for sputtering the indium tin zinc oxide film were polycrystalline indium tin oxide and polycrystalline zinc oxide. The sputtering time was 60 s. The sputtering power of the polycrystalline indium tin oxide target was set to 100 W, the sputtering power of the polycrystalline magnesium oxide target was set to 70 W, and the sputtering power of the polycrystalline zinc oxide target was set to 130 W.
[0054] 3) The polyimide substrate with the prepared active layer is placed in a patterned metal mask and fixed, and then a polycrystalline indium tin oxide target is used to deposit a polycrystalline indium tin oxide thin film with a thickness of 100 nm on the surface of the active layer as a source electrode and a drain electrode by direct current magnetron sputtering. The width of the channel between the source electrode and the drain electrode is 300 μm and the length is 100 μm, that is, the aspect ratio is 3:1, to form a source-drain electrode layer; the process parameters of the direct current magnetron sputtering are as follows: the sputtering chamber pressure is set to 0.5 Pa, the gas atmosphere is oxygen and argon, the flow rates are set to 3 sccm and 10 sccm respectively, the sputtering temperature is set to 30°C, the sputtering power of the polycrystalline indium tin oxide target is set to 100 W, and the sputtering time is set to 10 min;
[0055] 4) dropping n-octyltriethoxysilane into a tungsten boat, and then inverting the polyimide substrate with the source-drain electrode layer prepared on the tungsten boat, so that the source-drain electrode layer does not directly contact the n-octyltriethoxysilane, and then placing the tungsten boat in a culture dish and sealing it, and then placing the sealed culture dish in a vacuum oven at 120° C. for 2 hours to form a hydrophobic barrier layer with a thickness of 2 nm on the back channel surface of the active layer;
[0056] 5) 2 g of silicone resin TSE399-C (Maitu), 0.15 g of ultraviolet light absorber DHHB and 2 g of xylene were mixed, magnetically stirred at room temperature for 1 h, then allowed to stand for 1 h, and then spin-coated onto the surface of the hydrophobic barrier layer using a gel coater. The specific operation of spin coating was: first spin coating at 2000 rpm for 40 s, then spin coating at 3000 rpm for 40 s, and then drying to form a near-ultraviolet light blocking layer with a thickness of 200 nm on the surface of the hydrophobic barrier layer, thereby obtaining a flexible deep ultraviolet photosynaptic transistor.
[0057] Comparative Example 1:
[0058] A flexible deep ultraviolet photosynaptic transistor is identical to the flexible deep ultraviolet photosynaptic transistor of the embodiment except that the active layer of the three-layer structure is replaced by a "40 nm thick indium tin zinc oxide film (single-layer structure)". Performance test:
[0059] a) The electrical properties of the flexible deep ultraviolet photosynaptic transistors of Example 1 and Comparative Example 1 were tested using an Agilent 4155C semiconductor parameter analyzer, and the obtained transfer characteristic curves were as follows: Figure 2 and Figure 3 shown.
[0060] contrast Figure 2 and Figure 3 It can be seen that the flexible deep ultraviolet photosynaptic transistor of the embodiment exhibits good switching characteristics, has a high switching current ratio, the transfer characteristic curve does not show distortion such as a hump, and the turn-on voltage shows a certain degree of negative drift. This is because compared with the single-layer indium tin zinc oxide active layer, the surface carrier density of the three-layer structure active layer of indium tin magnesium oxide / indium tin zinc oxide / indium tin magnesium oxide will increase, so the deep ultraviolet photosynaptic transistor of the embodiment is a depletion-type device.
[0061] b) The output performance of the flexible deep ultraviolet photosynaptic transistors of Example 1 and Comparative Example 1 was tested using an Agilent 4155C semiconductor parameter analyzer. The output characteristic curves obtained were as follows: Figure 4 and Figure 5 shown.
[0062] Depend on Figure 4 and Figure 5It can be seen that the output characteristics of the flexible deep ultraviolet photosynaptic transistors of the embodiment and comparative example 1 both show good linear growth at low voltage density, without current crowding effect, and there is a clear difference between the linear region and the saturation region of the output curve, indicating that the active layers of both have good ohmic contact with the source / drain electrodes.
[0063] c) The response performance of the flexible deep ultraviolet photosynaptic transistors of Example 1 and Comparative Example 1 to a deep ultraviolet double pulse signal with a wavelength of 254 nm was tested in air with a relative humidity of 60%. The changes in the postsynaptic currents obtained were as follows: Figure 6 and Figure 7 shown.
[0064] Depend on Figure 6 and Figure 7 It can be seen that the postsynaptic current value of the flexible deep ultraviolet photosynaptic transistor in comparative example 1 is only 0.8nA, and the double pulse promotion index is 148%, while the postsynaptic current value of the flexible deep ultraviolet photosynaptic transistor in the embodiment is about 1500nA, and the double pulse promotion index is 229.5%, which are 1875 times and 1.55 times of the flexible deep ultraviolet photosynaptic transistor in comparative example 1 respectively.
[0065] In summary, since the active layer of the flexible deep ultraviolet photosynaptic transistor of the embodiment introduces a vertical electric field, the separation of photogenerated carriers can be accelerated, and the postsynaptic current value and the double pulse promotion index of the device are significantly higher than those of the flexible deep ultraviolet photosynaptic transistor of Comparative Example 1, indicating that the three-layer structure active layer of indium tin magnesium oxide / indium tin zinc oxide / indium tin magnesium oxide used in the present invention can significantly improve the pulse light response characteristics and photoelectric memory characteristics of the deep ultraviolet photosynaptic transistor.
[0066] Comparative Example 2:
[0067] A flexible deep ultraviolet photosynaptic transistor is exactly the same as the flexible deep ultraviolet photosynaptic transistor of the embodiment, except that the active layer of the three-layer structure is replaced by "an indium tin magnesium oxide film with a thickness of 10nm and an indium tin zinc oxide film with a thickness of 20nm stacked in sequence from bottom to top (double-layer structure)".
[0068] After testing (the testing method is the same as the embodiment), the response performance of the flexible deep ultraviolet photosynaptic transistor in this comparative example to the deep ultraviolet pulse signal with a wavelength of 254nm is reduced, the postsynaptic current value is about 900nA, and the double pulse promotion index is 180%. It can be seen that the active layer with a three-layer structure is more conducive to separating photogenerated carriers and realizing electron capture to enhance the response characteristics and memory performance of the synaptic transistor.
[0069] Comparative Example 3:
[0070] A flexible deep ultraviolet photoelectric synaptic transistor is identical to the flexible deep ultraviolet photoelectric synaptic transistor of the embodiment except that the ultraviolet light absorber DHHB is replaced by "ultraviolet absorber UV-328".
[0071] After testing (the testing method is the same as that in the embodiment), the flexible deep ultraviolet photosynaptic transistor of this comparative example has a pulse width of 100ms and a light intensity of 20μW / cm 2 The response current to the weak deep ultraviolet light pulse is 100nA, and the response to the interference signal (near ultraviolet light with a wavelength of 365nm) is basically unchanged. It can be seen that the ultraviolet light absorber DHHB has better ultraviolet light transmittance selectivity, which makes the deep ultraviolet photosynapse transistor have a higher signal-to-noise ratio.
[0072] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A flexible deep ultraviolet photosynaptic transistor, characterized in that: The composition includes a flexible substrate, a gate dielectric layer, an active layer, a source-drain electrode layer, a hydrophobic barrier layer and a near-ultraviolet light barrier layer which are stacked in sequence, and also includes a gate electrode which is arranged inside the gate dielectric layer and in contact with the flexible substrate; the composition of the active layer includes a first indium tin magnesium oxide layer, an indium tin zinc oxide layer and a second indium tin magnesium oxide layer which are stacked in sequence.
2. The flexible deep ultraviolet photosynaptic transistor according to claim 1, characterized in that: The thickness of the first indium tin magnesium oxide layer is 5nm-30nm; the thickness of the indium tin zinc oxide layer is 10nm-40nm; and the thickness of the second indium tin magnesium oxide layer is 5nm-30nm.
3. The flexible deep ultraviolet photosynaptic transistor according to claim 1 or 2, characterized in that: The flexible substrate is one of a flexible polyimide substrate, a flexible polyethylene terephthalate substrate and a flexible polyether substrate.
4. The flexible deep ultraviolet photosynaptic transistor according to claim 1 or 2, characterized in that: The gate dielectric layer is composed of one of neodymium aluminum oxide, aluminum oxide, silicon dioxide and zirconium oxide.
5. The flexible deep ultraviolet photosynaptic transistor according to claim 1 or 2, characterized in that: The gate electrode is composed of at least one of Al and Nd; the source electrode in the source-drain electrode layer is one of ITO electrode, Al electrode, Cu electrode, and Au electrode; the drain electrode in the source-drain electrode layer is one of ITO electrode, Al electrode, Cu electrode, and Au electrode.
6. The flexible deep ultraviolet photosynaptic transistor according to claim 1 or 2, characterized in that: The hydrophobic barrier layer is composed of at least one of n-octyltriethoxysilane, octadecyltrimethoxysilane and octadecyltrichlorosilane.
7. The flexible deep ultraviolet photosynaptic transistor according to claim 1 or 2, characterized in that: The near-ultraviolet light blocking layer comprises an optically transparent silicone resin and a near-ultraviolet light absorber.
8. A method for preparing a flexible deep ultraviolet photosynaptic transistor as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: 1) depositing a gate electrode and a gate dielectric layer in sequence on a single side of a flexible substrate; 2) depositing an indium tin magnesium oxide layer, an indium tin zinc oxide layer and an indium tin magnesium oxide layer on the surface of the gate dielectric layer in sequence to form an active layer; 3) depositing a source electrode and a drain electrode on the surface of the active layer to form a source-drain electrode layer; 4) placing the device obtained in step 3) in an atmosphere containing a hydrophobic substance to form a hydrophobic barrier layer; 5) Covering the surface of the hydrophobic barrier layer with a near-ultraviolet light blocking material to form a near-ultraviolet light blocking layer, thereby obtaining a flexible deep ultraviolet photosynaptic transistor.
9. An array substrate, characterized in that: A flexible deep ultraviolet photosynaptic transistor comprising any one of claims 1 to 7.
10. A neuromorphic computer, characterized in that A flexible deep ultraviolet photosynaptic transistor comprising any one of claims 1 to 7.
Citation Information
Patent Citations
Thin film transistor and manufacturing method thereof
CN104241393A
Inorganic synaptic transistor structure and manufacturing method thereof
CN111739935A
Preparation method of indium gallium zinc oxide-based multilayer structure thin film transistor
CN112599420A
Full-transparent thin film transistor device and preparation method thereof
CN115274833A
Zinc oxide-based solar-blind ultraviolet photoelectric detector and preparation method and application thereof
CN115274873A