An InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer
By adopting a folded quantum well layer structure in InGaN-based red LEDs, the problems of GaAs material compatibility and light attenuation are solved, the luminous efficiency and crystal quality of red LEDs are improved, and efficient red light emission is achieved, promoting the development of InGaN-based red LEDs. Development of light LED technology.
Patent Information
- Application Number
- CN202410815317.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-24
AI Technical Summary
GaAs materials have compatibility issues and light attenuation problems in the manufacturing of red LEDs, which increase production costs and limit the development of LED technology. InGaN-based red epitaxy technology faces limitations in material physical properties and manufacturing difficulties, especially in high In doping At higher concentrations, the crystal quality is affected and the carrier energy bands are distorted, affecting LED performance and production efficiency.
An InGaN-based red LED epitaxial film structure with a folded quantum well layer is used, including a sapphire patterned substrate, a composite buffer layer, a stress relief and porous structure generation layer, an N-type GaN layer circulation structure and a folded quantum well layer. Specific growth steps and parameter control achieve luminescence in the red light band.
It effectively improves the luminous wavelength and luminous efficiency of InGaN-based red LEDs, improves the overall crystal quality of GaN epitaxy, releases stress, improves product uniformity and production efficiency, and has good repeatability and stability.
Smart Images

Figure CN118380522B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor optoelectronic technology, in particular to an InGaN-based red light LED epitaxial film structure with a folded quantum well layer. Background Art
[0002] The core epitaxial material of red LEDs in the current market is mainly GaAs, which plays an important role in LED manufacturing. However, with the rapid development and widespread application of micro-LED technology and its various application fields, some problems have begun to surface. In particular, the compatibility issue between GaAs materials and GaN materials widely used in blue-green LEDs is gradually becoming a key factor restricting the further development of the industry.
[0003] This problem is not only reflected in the difference in physical and chemical properties of the two materials, but also in the insurmountable gap between them in terms of process integration and performance matching. At the same time, the manufacturing process of GaAs materials is quite complicated, involving multiple precision process steps, which undoubtedly increases production costs and also affects the yield rate of products. The decline in yield rate not only means a waste of resources, but also affects the profitability of enterprises.
[0004] In addition, the light attenuation problem of GaAs on small-sized LED chips cannot be ignored. Although researchers and engineers have tried many methods to solve this problem, they have not yet found an economical and efficient solution. The existence of this problem not only affects the performance and service life of LED products, but also limits the further development of LED technology to a certain extent.
[0005] In this context, InGaN-based red light epitaxy technology has begun to attract widespread attention in the industry. This technology is seen as a potential replacement for GaAs and a core technology for the next generation of red light LEDs. Its main advantage is that it is expected to improve the uniformity of materials and devices, thereby improving production efficiency. However, this technology is not without challenges.
[0006] InGaN-based red LED epitaxy technology faces limitations in the physical properties of the material. In particular, when trying to achieve high In doping concentrations, the quality of the crystal is often affected and the carrier energy band is distorted. These problems not only affect the performance of the LED, but also increase the difficulty and cost of manufacturing.
[0007] Therefore, in order to promote the development of InGaN-based red LED epitaxial technology, researchers are working to improve the overall crystal quality of GaN epitaxy and find effective ways to release the internal stress in the material. These efforts are not only related to the performance and production cost of LED products, but also the key to driving the entire LED industry forward. It can be said that solving these problems has become the primary task of developing InGaN-based red LED epitaxial thin film layers. Summary of the invention
[0008] The purpose of the present invention is to provide an InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer to solve the above technical problems. The present invention further increases the light emission wavelength of the LED thin film layer through a special folded quantum well layer design to achieve light emission in the red light band.
[0009] The technical solution of the present invention is as follows:
[0010] An InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer, comprising:
[0011] Sapphire patterned substrate;
[0012] A composite buffer layer is disposed on the sapphire patterned substrate;
[0013] uGaN (undoped gallium nitride) layer, disposed on the composite buffer layer;
[0014] A stress release and porous structure generation layer is arranged on the uGaN layer, and includes a multilayer structure of u-InGaN (indium gallium nitride not doped with Si) / H2 etching / GaN, and is used to release stress and form a porous structure;
[0015] A GaN cap layer, disposed on the stress release and porous structure generation layer;
[0016] An N-type GaN layer cyclic structure is arranged on the GaN cap layer and forms a concave-convex surface by a low-temperature growth method;
[0017] A third stress release layer is provided on the N-type GaN layer cycle structure;
[0018] A folded quantum well layer is arranged on the third stress release layer, and is a cyclic structure of an InN layer, a quantum well, and a quantum well barrier, wherein the number of cycles is controlled at 5-20, the thickness of the InN layer is controlled at 0.5-1.0 nm, the quantum well is an InGaN with a thickness controlled at 2-3 nm, and the doping concentration of In is controlled at 30%-35%, and the quantum well barrier includes Barrier1 and Barrier2, wherein Barrier1 is an AlGaN with a thickness controlled at 1-2 nm, and the Al doping concentration is controlled at 20%-25%, and Barrier2 is a GaN with a thickness controlled at 2-3 nm;
[0019] An LT-PGaN (low temperature P-type gallium nitride) layer, an electron blocking layer (EBL), a HT-PGaN (high temperature P-type gallium nitride) layer and a P-type contact layer (P-Contact layer) are sequentially arranged on the folded quantum well layer;
[0020] The design of the folded quantum well layer enables the peak wavelength of the LED to be controlled within the red light band between 600nm and 620nm.
[0021] The composite buffer layer comprises an AlN material composite buffer layer and a low-temperature GaN material composite buffer layer which are arranged in sequence.
[0022] During the growth of the stress release and porous structure generation layer, H2 is used to etch the surface and shallow surface InN materials to form a micro-pore structure.
[0023] The N-type GaN layer cycle structure includes a Si-doped N-type GaN layer and a Si-doped N-type InGaN layer, and the cycle number is controlled at 10-15; the thickness of each Si-doped N-type GaN layer is controlled at 0.05-0.1um, and the Si doping concentration is controlled at 1.0E19-1.5E19; the thickness of each Si-doped N-type InGaN layer is controlled at 0.1-0.2um, and the Si doping concentration is controlled at 1.0E19-1.5E19.
[0024] The peak wavelength of the light emission of the InGaN-based red light LED epitaxial thin film structure with the folded quantum well layer is controlled in the red light band between 600nm and 620nm.
[0025] The preparation method of the InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer includes specific growth steps, material selection and parameter control; the growth steps include the sequential growth of a composite buffer layer, a uGaN layer, a stress release and porous structure generation layer, a GaN cap layer, an NGaN layer cyclic structure, a third stress release layer, a multi-quantum well light-emitting layer, an LT-PGaN layer, an EBL, a HT-PGaN layer and a P-Contact layer; by adjusting fine parameters, the light emission peak wavelength of the LED chip is controlled to be in the red light band between 600nm and 620nm.
[0026] In the present invention, the design of the folded quantum well layer is the key innovation point, and luminescence in the red light band is achieved through specific growth steps and parameter control: the design of the stress release and porous structure generation layer improves the overall stacking quality of the GaN epitaxy and releases stress; the N-type GaN layer cyclic structure adopts a low-temperature growth method to further release stress and form a concave-convex surface; the multi-quantum well light-emitting layer includes a fine structure of Well and Barrier, and an InN layer for increasing the effective In doping concentration of the Well; the design of the LT-PGaN layer, the EBL layer, the HT-PGaN layer and the P-Contact layer optimizes the electron blocking and hole injection effects.
[0027] The beneficial effects of the present invention are as follows: through the design of the folded quantum well layer, the luminous wavelength and luminous efficiency of the InGaN-based red light LED are effectively improved; at the same time, through the design of a special stress release and porous structure generation layer, the overall stacking quality of the GaN epitaxy is effectively improved and the stress is released; in addition, the structure of the present invention also has good repeatability and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the structure of the complete epitaxial stacking crystal of the present invention.
[0029] Figure 2 Shown is a schematic diagram of the u-InGaN / H2 etching / GaN multilayer structure.
[0030] Figure 3 This is the TEM characterization image of the u-InGaN / H2 etching / GaN multilayer structure after the growth is completed with an actual design cycle number of 20 loops.
[0031] Figure 4 It shows that the u-InGaN / H2 etching / GaN multilayer porous structure has an impact on the emission wavelength of the LED structure.
[0032] Figure 5 It is a schematic diagram of the cyclic structure of N-type GaN layers.
[0033] Figure 6 Shown are the fine structure and specific parameters of the multi-quantum well layer.
[0034] Figure 7 It is a characterization of the morphology of the folded quantum well actually grown in the present invention.
[0035] Figure 8 Shown are the PL spectrum with a peak wavelength of 616 nm and the red light emission during EL point measurement. DETAILED DESCRIPTION
[0036] Preferred embodiments of the present invention are given below in conjunction with the accompanying drawings to illustrate the technical solutions of the present invention in detail.
[0037] Example
[0038] The present invention provides an InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer (such as Figure 1 As shown in the figure), it effectively solves the problems existing in the existing red light LED technology through special structural design and realizes high-efficiency and high-quality red light emission.
[0039] The specific implementation steps are as follows:
[0040] Prepare substrate 1: Select sapphire patterned substrate as the substrate. This substrate has good thermal stability and mechanical strength and is suitable for LED epitaxial growth.
[0041] Growth of composite buffer layer 2: First, a composite buffer layer of AlN material is grown on the substrate using PVD evaporation technology, and its thickness is controlled between 15-30nm. This layer is mainly used to alleviate the lattice mismatch between the substrate and the subsequent epitaxial layer. Next, a low-temperature GaN material composite buffer layer is grown on the AlN buffer layer using MOCVD technology, with a thickness between 10-30nm and a growth temperature maintained at 700-850℃. This step helps to further improve the bonding quality between the epitaxial layer and the substrate.
[0042] uGaN layer 3 growth: A non-doped GaN layer is grown on top of the composite buffer layer. This layer first fills the substrate pattern height through a 3D roughening layer, and then grows a capping layer to make the GaN film surface flat, with the overall thickness controlled between 2.5-3.5μm.
[0043] Growth of stress release and porous structure generation layer 4: The first group of stress release and porous structure generation layers are grown on top of the flat uGaN layer. The detailed structures are: u-InGaN / H2 etching / GaN, with a thickness range of InGaN (2-6nm). After the InGaN growth is completed, a 150-300 second pause layer is set, and the atmosphere is switched to 50% N2 / H2, and H2 is used to etch the surface and shallow InN materials to form a micro-pore structure. After that, a layer of GaN (2-4nm) is grown to space the InGaN and enlarge the size of the porous cavity formed by H2 etching. The growth temperature is set to 850-950℃, and the InGaN layer growth temperature is set to 720-780℃. This step can be repeated 5 to 20 times to further enhance the stress release effect. Figure 2 The figure shows a schematic diagram of a u-InGaN / H2etching / GaN multilayer structure. This special structure with micro-pores formed by H2 etching helps to release stress in the epitaxial layer. Figure 3 This is the TEM characterization image of the u-InGaN / H2etching / GaN multilayer structure after growth, with the actual design of 20 loops, the initial design value of u-InGaN (4.5nm), and the initial design value of GaN (2.0nm). The average thickness of the u-InGaN single layer is 4.5nm, and the average thickness of the GaN layer is 2.2nm. Compared with the initial design value, the relative thickness of the u-InGaN layer is thinner, and the GaN is relatively thicker. This is mainly caused by the H2 etching layer corroding the InN in the u-InGaN, but the micro-porous morphology cannot be clearly presented at this characterization accuracy. In order to prove that the u-InGaN / H2 etching / GaN multilayer porous structure designed in this scheme has an impact on the emission wavelength of the LED structure, a design is arranged to remove the u-InGaN / H2 etching / GaN multilayer porous structure for growth, as shown in part (a) of Figure 4. It can be clearly seen that the peak wavelength WLP after removing the u-InGaN / H2 etching / GaN multilayer porous layer is about 550nm, and its luminous color is obvious yellow light, but the peak wavelength WLP of the u-InGaN / H2etching / GaN multilayer porous layer structure is about 600nm, and its luminous color is red light, as shown in part (b) of Figure 4.
[0044] uGaN cap layer 5 growth: After the stress release layer and the porous layer cyclic structure growth are completed, a uGaN cap layer with a thickness of 0.2-0.5 μm is grown to isolate the entry of doping of the upper structural layer.
[0045] Growth of N-type GaN layer cyclic structure 6: On the flat uGaN surface layer, grow an N-type GaN layer cyclic structure. This structure is entirely Si-doped N-type GaN layer, which uses a low-temperature growth method to further release stress and form a concave-convex surface, providing a substrate for the subsequent folded quantum well layer. Among them, the cyclic structure is GaN (Si) / InGaN (Si), its single cycle thickness is controlled at 0.15-0.3μm, the In doping concentration is controlled at 5E18-2E19, the number of cycles is controlled at 10-15, the Si doping concentration is 1.0E19-1.5E19, the overall N-type GaN layer cyclic structure thickness is controlled in the range of 1.5-3.0μm, and the overall growth temperature is controlled at 850℃ to 950℃; its structure is as follows Figure 5 shown.
[0046] Growth of superlattice structure 7: A layer of low Si doping (1.0 E19-2.0E19) n-GaN is grown on top of the N-type GaN cyclic structure layer as a barrier and low In (5.0 E18-2.0E19) and Si doping (doping concentration 1.0 E19-2.0E19) n-InGaN is grown as a Well superlattice structure as the third stress release layer, with an overall thickness range of 0.5-1.0μm.
[0047] Growth of folded quantum well layer 8: Next, the folded quantum well layer is grown. The fine structure and specific parameters of the folded quantum well layer are as follows: Figure 6 As shown, a folded quantum well structure is designed to increase the effective In doping concentration of the Well. The folded quantum well layer is a cyclic structure of an InN layer, a quantum well, and a quantum well barrier. In this embodiment, the number of cycles is controlled at 5, the thickness of the InN layer is controlled at 0.5nm, the thickness of the quantum well is controlled at 2-3nm InGaN, and the In doping concentration is controlled at 35%. The quantum well barrier includes Barrier1 and Barrier2, wherein Barrier1 is AlGaN with a thickness controlled at 1-2nm, the Al doping concentration is controlled at 25%, and Barrier2 is GaN with a thickness controlled at 2-3nm. The InN layer can increase the effective In doping concentration in the quantum well InGaN. The morphology of the folded quantum well actually grown in this embodiment is characterized as shown in the figure. Figure 7 As shown in part (a) of Figure 7, the actual average value of the Well grown is 2.36nm=(23+20+24+22+29)Å / 5, and the actual average thickness of the Barrier is 3.84nm=(47+34+43+35+33)Å / 5. There are some differences between these two characterization values and the design values. In addition to the fluctuation of the characterization error, it is also caused by the difference between the actual thickness of the quantum well grown in a folded shape and when it grows on a flat C crystal surface. Part (b) of Figure 7 shows the TEM structure of the folded multi-quantum well at a wide viewing angle.
[0048] Subsequent layer structure growth: After the multi-quantum well layer is grown, the low-temperature PGaN layer 9, the electron blocking layer EBL 10, the high-temperature PGaN layer 11 and the PGaN contact layer 12 are grown in sequence. These layer structures help to improve the luminous efficiency and stability of the LED. Among them, the low-temperature P-type GaN layer (LT-PGaN) has a thickness range of 15-30nm, wherein the Mg doping concentration is 5E19-1E21, the In doping concentration is 1E18-1E19, and the Al doping concentration is 1E18-5E18; the electron blocking layer EBL has a thickness of 20-40nm, and the Al doping adopts a gradual change, and its doping concentration gradually changes from 1E21 to 1E19; the high-temperature P-type GaN layer (HT-PGaN) has a thickness of 15-30nm, and the Mg doping concentration is 1E20-1E21; the PGaN contact layer (P-Contact layer) with a high Mg component has a thickness of 5-10nm, and the Mg doping concentration is 1E21-2E21; the N-type GaN layer is etched by ICP to produce a circular structure electrode interface, and an ITO transparent conductive film 13 is evaporated on the PGaN contact layer, and its thickness can be controlled in the range of 30-110nm;
[0049] Electrode fabrication and testing: Finally, the LED chip electrodes (p-PAD1201, n-PAD601) and other process layer structures are fabricated and spot tested. By adjusting fine parameters, the peak wavelength of the InGaN-based red LED of the present invention can be controlled within the red light band of 600nm~620nm, showing excellent photoelectric performance. Figure 8 Shown are the PL spectrum with a peak wavelength of 616 nm and the red light emission during EL point measurement.
[0050] In summary, the present invention successfully achieves high-efficiency and high-quality red light emission through the special folded quantum well layer design and other epitaxial layer structure optimization. This technical solution provides new ideas and methods for the development of red light LEDs, and has important application value and development prospects.
Claims
1. An InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer, characterized in that: include: Sapphire patterned substrate; A composite buffer layer is disposed on the sapphire patterned substrate; A uGaN layer, disposed on the composite buffer layer; A stress release and porous structure generation layer is arranged on the uGaN layer, and includes a multilayer structure of u-InGaN / H2 etching / GaN, and is used to release stress and form a porous structure; A GaN cap layer, disposed on the stress release and porous structure generation layer; An N-type GaN layer cyclic structure is arranged on the GaN cap layer and forms a concave-convex surface by a low-temperature growth method; A third stress release layer is provided on the N-type GaN layer cycle structure; A folded quantum well layer is arranged on the third stress release layer, and is a cyclic structure of an InN layer, a quantum well, and a quantum well barrier, wherein the number of cycles is controlled at 5-20, the thickness of the InN layer is controlled at 0.5-1.0 nm, the quantum well is an InGaN with a thickness controlled at 2-3 nm, and the doping concentration of In is controlled at 30%-35%, and the quantum well barrier includes Barrier1 and Barrier2, wherein Barrier1 is an AlGaN with a thickness controlled at 1-2 nm, and the Al doping concentration is controlled at 20%-25%, and Barrier2 is a GaN with a thickness controlled at 2-3 nm; The LT-pGaN layer, the EBL, the HT-pGaN layer and the P-type contact layer are sequentially arranged on the folded quantum well layer; The design of the folded quantum well layer enables the peak wavelength of the LED to be controlled within the red light band between 600nm and 620nm.
2. The InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer according to claim 1, characterized in that: The composite buffer layer comprises an AlN material composite buffer layer and a low-temperature GaN material composite buffer layer which are arranged in sequence.
3. The InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer according to claim 1, characterized in that: The stress release and porous structure generation layer includes 5-20 layers of u-InGaN / H2 etching / GaN structure.
4. The InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer according to claim 1, characterized in that: The N-type GaN layer cycle structure comprises a Si-doped N-type GaN layer and a Si-doped N-type InGaN layer, and the cycle number is controlled to be 10-15.
5. The InGaN-based red light LED epitaxial thin film structure with a folded quantum well layer according to claim 1, characterized in that: Its luminous peak wavelength is controlled in the red light band between 600nm and 620nm.