A process for producing medium chromium cast iron floating oil seal by centrifugal casting

Through medium-chromium cast iron materials and centrifugal casting technology, the problems of high consumption of rare and precious metals and poor inner diameter roughness in floating oil seal production are solved, and efficient and low-cost floating oil seal production are achieved, with performance reaching or exceeding high-chromium cast iron and Ni-hard series.

CN118385502BActive Publication Date: 2024-11-05YANTAI YUANNONG SEALING TECH CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410865832.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-05
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

In the production process of existing floating oil seals, high chromium cast iron and Ni-hard series high nickel cast iron materials need to be added with high content of rare precious metals, resulting in high cost and limited use performance. The centrifugal casting process has poor inner diameter roughness and many impurities. question.

Method used

The medium-chromium cast iron material is used to produce floating oil seals through centrifugal casting process, including smelting alloy raw materials in an intermediate frequency furnace, controlling the iron liquid temperature and centrifugal casting, rapid filling with centrifugal force, followed by rough processing and sealing surface grinding to reduce impurities and sand eye Defects, reduce the demand for rare and precious metals.

Benefits of technology

It realizes efficient production of medium-chromium cast iron floating oil seals, reduces rare and precious metal consumption, improves wear resistance and sealing performance, reduces production defects, is low in cost and better than traditional high-chromium cast iron and Ni-hard series high-nickel cast iron.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a process method for producing a medium-chromium cast iron floating oil seal by centrifugal casting, and relates to the technical field of centrifugal casting. The medium-chromium cast iron floating oil seal of the invention adopts a centrifugal casting method, and the product is fast in filling, suitable for large-scale continuous production, and has high production efficiency. At the same time, the molten iron filling time and filling flow path of the medium-chromium cast iron are short, and the probability of impurities being involved in the casting is extremely small, thereby reducing defects such as sand holes and slag inclusions, and after the filling is completed, the outer surface of the casting is rapidly cooled and crusted, so the outer surface roughness of the casting is good, and by adding the medium-chromium cast iron, it is not necessary to add a high content of rare and precious metals to meet the wear resistance and sealing performance of the floating oil seal, thereby reducing the demand and loss of rare and precious metals, and the medium-chromium cast iron floating oil seal produced within the set centrifugal parameter range is tested for its HV microhardness and the metallographic structure of each part is observed, and there is no hardness unevenness and segregation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of centrifugal casting, in particular to a process for producing a medium chromium cast iron floating oil seal by centrifugal casting. Background Art

[0002] At present, the main materials of floating oil seals produced by casting technology are high chromium cast iron and Ni-hard series high nickel cast iron. In order to achieve high wear resistance and good sealing performance, it is necessary to add high content of rare and precious metals such as molybdenum, nickel, tungsten or vanadium for alloying to improve hardenability, refine grains or strengthen the matrix. As a basic component in the engineering machinery industry, floating oil seals are widely used and used in large quantities, so the consumption of rare and precious metals is very large. The content of rare and precious metals such as molybdenum, nickel, tungsten or vanadium in the earth's crust is extremely rare and non-renewable, and the price is extremely expensive, resulting in a high cost of floating oil seals.

[0003] In terms of production technology: Cast floating oil seals are the main manufacturing method for floating oil seals due to the uniformity of casting materials and excellent product stability. The production process of cast floating oil seals is divided into gravity casting and centrifugal casting according to the filling method. Centrifugal casting is a more commonly used method. Centrifugal casting refers to the technology and method of injecting high-temperature molten iron into a high-speed rotating mold so that the molten iron fills the mold and forms a casting under the action of centrifugal force. Due to the high centrifugal force, the filling speed of the molten iron is faster, the grain size of the casting is finer, the density is better, and the casting has better wear resistance than gravity casting. When centrifugally casting the existing floating oil seal, the inner diameter of the centrifugal casting is naturally formed and subjected to a large centrifugal force. Therefore, during the cooling process, the centrifugal force will cause the inner diameter to have a shallow depression, and the molten iron residue will also float to the inner diameter under the action of centrifugal force. Therefore, the roughness of the inner diameter will be poor, and there will be more residue, which needs to be processed and improved.

[0004] For the sustainable development of the industry, it is necessary to find alternative materials for floating oil seal application materials such as high chromium cast iron and Ni-hard series high nickel cast iron. On the one hand, there is no need to use high content of rare precious metal alloying. On the other hand, the performance of existing floating oil seals using rare precious metals must be achieved or exceeded. At the same time, the defects of existing casting processes can be alleviated during casting. Summary of the invention

[0005] The purpose of the present invention is to solve the above problems and provide a process for producing medium chromium cast iron floating oil seal by centrifugal casting.

[0006] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:

[0007] A process for producing a medium chromium cast iron floating oil seal by centrifugal casting comprises the following steps:

[0008] S1. Prepare the ingredients according to the standard requirements of medium chromium cast iron, put the prepared alloy raw materials into a medium frequency furnace for smelting, detect the castings with a spectrometer after smelting and adjust the composition of the molten iron to be within the standard range of medium chromium cast iron;

[0009] S2, purify the molten iron according to the operating process, detect the temperature of the molten iron with a contact temperature measuring gun, control the temperature of the molten iron to 1480-1620°C, and then pour it out of the furnace;

[0010] S3, using a centrifugal process method for casting, specifically: clean the impurities in the mold, the top mold mechanism falls back, the mold falls and closes, start the centrifugal device, scoop the molten iron with a crucible, and directly pour the specified volume of molten iron into the rotating mold cavity to form a casting mold. Under the action of centrifugal force, the molten iron quickly fills the mold outward from the pouring point, then the timer is started, and after the timing is completed, the centrifugal device is stopped. After the device stops steadily, the top mold mechanism is lifted, the mold is separated from the casting, and the medium chromium cast iron floating oil seal blank is obtained, and the impurities in the mold are cleaned to prepare for the next centrifugal casting;

[0011] S4. The medium chrome cast iron floating oil seal blank is subjected to a process of rough machining, inner spherical grinding and sealing surface grinding to meet the corresponding size requirements and the surface roughness and flatness required for sealing performance, so as to obtain a medium chrome cast iron floating oil seal semi-finished product; the medium chrome cast iron floating oil seal semi-finished product is cleaned and inspected to obtain a medium chrome cast iron floating oil seal finished product.

[0012] Furthermore, the weight percentage content of the main elements of the medium chromium cast iron is in the range of C2.8-3.8; Si1.0-2.5; Cr6.0-12.0, Mn0.2-1.0; and the rest is Fe.

[0013] Furthermore, the medium chromium cast iron contains not only main elements but also auxiliary elements, and the weight percentage of the auxiliary elements is less than 1.0%.

[0014] Furthermore, the auxiliary element is a rare element.

[0015] Furthermore, the auxiliary element is an element of the Re group.

[0016] Furthermore, the mold material is graphite.

[0017] Furthermore, the mold is made of metal.

[0018] Furthermore, the Rockwell hardness of the medium chromium cast iron floating oil seal is HRc55-65.

[0019] Furthermore, the rotation speed of the mold in the centrifugal device is 300-1500rpm.

[0020] Furthermore, the centrifugation time of the centrifugal device is 20-180 seconds.

[0021] The beneficial effects of the present invention are as follows:

[0022] 1. The medium chromium cast iron floating oil seal of the present invention adopts centrifugal casting, the product has fast filling, is suitable for large-scale continuous production, and has high production efficiency. At the same time, the molten iron filling time and filling flow path of the medium chromium cast iron are short, and the probability of impurities being involved in the casting is extremely small, thereby reducing defects such as sand holes and slag inclusions. After the filling is completed, the outer surface of the casting is quickly cooled and crusted, so the outer surface roughness of the casting is better.

[0023] 2. The present invention can meet the wear resistance and sealing performance of the floating oil seal by adding medium chromium cast iron, without adding a high content of rare metals, thereby reducing the demand and loss of rare metals.

[0024] 3. The medium chromium cast iron floating oil seal produced by the present invention within the set centrifugal parameter range is tested for its HV microhardness and its metallographic structure at various parts is observed, and no hardness unevenness or segregation is found.

[0025] 4. The present invention adopts centrifugal casting. From the circumferential direction, the stationary molten iron is injected into the rotating cavity. The inertia and centrifugal force drive the medium chromium cast iron liquid to replenish the outer diameter of the mold. The exposed parts dissipate heat evenly, the temperature gradient difference of each part is small, and the roundness stability of the casting is good. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below.

[0027] A process for producing a medium chromium cast iron floating oil seal by centrifugal casting according to a preferred embodiment of the present invention will be described in detail below.

[0028] A process for producing a medium chromium cast iron floating oil seal by centrifugal casting comprises the following steps:

[0029] S1. Prepare the ingredients according to the standard requirements of medium chromium cast iron, put the prepared alloy raw materials into the medium frequency furnace for smelting, use a spectrometer to detect the castings after smelting and adjust the composition of the molten iron to within the standard range of medium chromium cast iron:

[0030] (1) The weight percentage content of its main elements ranges from C2.8-3.8; Si1.0-2.5; Cr6.0-12.0, Mn0.2-1.0; the rest is Fe;

[0031] (2) In addition to the main elements, it may contain one or more of the rare and precious elements such as Mo, Ni, W, Co, V, Ti, Nb or Re group elements;

[0032] (3) If it contains rare and precious elements such as Mo, Ni, W, Co, V, Ti, Nb or Re group elements, the weight percentage of the content is less than 1.0%;

[0033] S2, purify the molten iron according to the operating process, detect the temperature of the molten iron with a contact temperature measuring gun, control the temperature of the molten iron to 1480-1620°C, and then pour it out of the furnace;

[0034] S3, using the centrifugal process method for pouring, specifically: clean the impurities in the mold, the top mold mechanism falls back, the mold falls and closes, start the centrifugal device, scoop the molten iron with a crucible, and pour the specified volume of molten iron directly into the graphite mold or metal mold cavity rotating at 300-1500rpm to form a casting mold. Under the action of centrifugal force, the molten iron quickly fills the mold outward from the pouring point. Then the timer starts, and the centrifugal device runs for 20-180 seconds. After the timing is completed, the centrifugal device stops. After the device stops steadily, the top mold mechanism is lifted, the mold is separated from the casting, and the medium chromium cast iron floating oil seal blank is obtained. Clean the impurities in the mold and prepare for the next centrifugal casting;

[0035] S4. The medium chrome cast iron floating oil seal blank is subjected to a process of rough machining, inner spherical grinding and sealing surface grinding to meet the corresponding size requirements and the surface roughness and flatness required for sealing performance, so as to obtain a medium chrome cast iron floating oil seal semi-finished product; the medium chrome cast iron floating oil seal semi-finished product is cleaned and inspected to obtain a medium chrome cast iron floating oil seal finished product.

[0036] The medium chromium cast iron floating oil seal produced within the centrifugal parameter range set by the present invention is tested for its HV microhardness and its metallographic structure at various parts is observed, and there is no hardness unevenness and segregation. The Rockwell hardness of the medium chromium cast iron floating oil seal is HRc55-65;

[0037] The medium chromium cast iron floating oil seal adopts centrifugal casting, and the product has fast filling, which is suitable for large-scale continuous production and high production efficiency. At the same time, the molten iron filling time and filling flow path of the medium chromium cast iron are short, and the probability of impurities being involved in the casting is extremely small, thus reducing defects such as sand holes and slag inclusions. After the filling is completed, the outer surface of the casting is quickly cooled and crusted, so the outer surface roughness of the casting is better. In other words, the medium chromium cast iron floating oil seal combined with centrifugal casting can reduce the defects of existing floating oil seals such as sand holes and slag inclusions during centrifugal casting;

[0038] By adding medium chromium cast iron, it is not necessary to add a high content of rare metals to meet the wear resistance and sealing performance of the floating oil seal, reducing the demand and loss of rare metals. Medium chromium cast iron is currently not used in the floating oil seal industry. It is a white cast iron with a medium chromium alloy content. Chromium, as the main alloying element, plays a role in whitening and forming wear-resistant iron-chromium carbide in cast iron. The chromium element comes from medium carbon ferrochrome FeCr60, which has a lower raw material price and is easier to obtain. It does not need to use a high content of rare metals for alloying, so the material cost is lower. The lower cost of medium chromium cast iron, combined with the advantages of centrifugal casting, can achieve or exceed the performance of high chromium cast iron or Ni-hard series high nickel cast iron floating oil seals, and may become the main material for floating oil seals in the future. Embodiment 1

[0039] This embodiment provides a medium chromium cast iron material, which includes the following alloy element components C: 2.86%, Si: 1.6%, Mn: 0.9%, Cr: 7.3%, and the balance is Fe and unavoidable impurities;

[0040] This embodiment also provides a floating oil seal made of the medium chromium cast iron material. The manufacturing process of the floating oil seal is as follows:

[0041] (1) Place the prepared alloy raw materials into a medium frequency furnace for smelting;

[0042] (2) When the molten iron in step (1) reaches 1580° C., a slag remover is added to remove the slag, and then the molten iron is taken out of the furnace;

[0043] (3) When the molten iron in step (2) reaches 1560° C., the molten iron is directly poured into a graphite mold cavity rotating at 800 rpm by a centrifugal process to form a mold. After centrifugation for 30 seconds, the rotation is stopped, and the mold is demolded to form a medium chromium cast iron floating seal ring blank;

[0044] (4) The rough machining, inner spherical grinding and sealing surface grinding process is performed on the medium chromium cast iron floating oil seal blank to meet the corresponding size requirements and achieve the surface roughness and flatness required for sealing performance, thereby obtaining a medium chromium cast iron floating oil seal semi-finished product; the medium chromium cast iron floating oil seal semi-finished product is cleaned and inspected to obtain a medium chromium cast iron floating oil seal finished product. Embodiment 2

[0045] The present embodiment provides a medium chromium cast iron material, which includes the following alloying element components in mass percentage: C3.3%, Si1.8%, Mn0.7%, Cr9.3%, Re0.21%, and the balance is Fe and unavoidable impurities;

[0046] This embodiment also provides a floating oil seal made of the medium chromium cast iron material. The manufacturing process of the floating oil seal is as follows:

[0047] (1) Place the prepared alloy raw materials into a medium frequency furnace for smelting;

[0048] (2) When the molten iron in step (1) reaches 1580° C., a slag remover is added to remove the slag, and then the molten iron is taken out of the furnace;

[0049] (3) When the molten iron in step (2) reaches 1560° C., the molten iron is directly poured into a graphite mold cavity rotating at 800 rpm by a centrifugal process to form a mold. After centrifugation for 30 seconds, the rotation is stopped, and the mold is demolded to form a medium chromium cast iron floating seal ring blank;

[0050] (4) The rough machining, inner spherical grinding and sealing surface grinding process is performed on the medium chromium cast iron floating oil seal blank to meet the corresponding size requirements and achieve the surface roughness and flatness required for sealing performance, thereby obtaining a medium chromium cast iron floating oil seal semi-finished product; the medium chromium cast iron floating oil seal semi-finished product is cleaned and inspected to obtain a medium chromium cast iron floating oil seal finished product. Embodiment 3

[0051] The present embodiment provides a medium chromium cast iron material, which includes the following alloy element components C: 3.6%, Si: 2.1%, Mn: 0.4%, Cr: 11.2%, Nb: 0.25%, Mo: 0.16%, Re: 0.21%, and the balance is Fe and unavoidable impurities;

[0052] This embodiment also provides a floating oil seal made of the medium chromium cast iron material. The manufacturing process of the floating oil seal is as follows:

[0053] (1) Place the prepared alloy raw materials into a medium frequency furnace for smelting;

[0054] (2) When the molten iron in step (1) reaches 1580° C., a slag remover is added to remove the slag, and then the molten iron is taken out of the furnace;

[0055] (3) When the molten iron in step (2) reaches 1560° C., the molten iron is directly poured into a graphite mold cavity rotating at 800 rpm by a centrifugal process to form a mold. After centrifugation for 30 seconds, the rotation is stopped, and the mold is demolded to form a medium chromium cast iron floating seal ring blank;

[0056] (4) The rough machining, inner spherical grinding and sealing surface grinding process is performed on the medium chromium cast iron floating oil seal blank to meet the corresponding size requirements and achieve the surface roughness and flatness required for sealing performance, thereby obtaining a medium chromium cast iron floating oil seal semi-finished product; the medium chromium cast iron floating oil seal semi-finished product is cleaned and inspected to obtain a medium chromium cast iron floating oil seal finished product.

[0057] Comparative Example 1. This comparative example provides a high chromium cast iron material, which includes the following alloying element components in percentage by mass: C: 3.5%; Si: 1.8%; Mn: 0.6%; Cr: 14.9%; Mo: 2.1%; Ni: 1.1%; the balance is Fe and unavoidable impurities;

[0058] This comparative example also provides a floating oil seal made of the high chromium cast iron material, and the manufacturing method of the floating oil seal is as follows:

[0059] (1) Place the prepared alloy raw materials into a medium frequency furnace for smelting;

[0060] (2) When the molten iron in step (1) reaches 1540° C., a slag remover is added to remove the slag, and then the molten iron is taken out of the furnace;

[0061] (3) When the molten iron in step (2) reaches 1520° C., it is directly poured into a casting mold that has been pre-molded with a rubber mold and assembled with coated sand to form a casting mold, and after natural cooling, it is divided into boxes to form a floating seal ring blank;

[0062] (4) The floating oil seal blank is subjected to a process of rough machining, quenching heat treatment, inner spherical surface grinding, and sealing surface grinding to meet the corresponding size, surface roughness, and flatness requirements to obtain a floating oil seal semi-finished product; the floating oil seal semi-finished product is cleaned and inspected to obtain a floating oil seal finished product.

[0063] Comparative Example 2: This comparative example provides a high-nickel cast iron material, which includes the following alloy element components in percentage by mass: C: 3.5%; Si: 2.0%; Mn: 0.6%; Cr: 2.6%; Mo: 0.03%; Ni: 3.6%; the balance is Fe and unavoidable impurities;

[0064] This comparative example also provides a floating oil seal made of the high-nickel cast iron material, and the manufacturing method of the floating oil seal is as follows:

[0065] (1) Place the prepared alloy raw materials into a medium frequency furnace for smelting;

[0066] (2) When the molten iron in step (1) reaches 1560° C., a slag remover is added to remove the slag, and then the molten iron is taken out of the furnace;

[0067] (3) When the molten iron in step (2) reaches 1540° C., it is directly poured into the cavity of a rotating graphite mold to form a mold, and after centrifugal rotation for 30 seconds, the mold is separated to form a floating seal ring blank;

[0068] (4) The floating oil seal blank is subjected to a process of rough machining, inner spherical grinding, and sealing surface grinding to meet the corresponding size, surface roughness, and flatness requirements to obtain a floating oil seal semi-finished product; the floating oil seal semi-finished product is cleaned and inspected to obtain a floating oil seal finished product.

[0069] The floating oil seals obtained from Examples 1-3 and Comparative Examples 1-2 were subjected to hardness testing and a running-in wear test of 168 hours of continuous operation. During the test, the sealing performance, temperature change, torque and pressure change of the floating oil seals were observed to be good, and no abnormalities were found on the sealing contact surfaces after disassembly inspection. The wear rate of each group was calculated by the weight loss method, and its service life was estimated. The test results are shown in Table 1.

[0070]

[0071] Compared with Comparative Examples 1 and 2, when the PV values ​​of Examples 1, 2 and 3 are similar or higher than the latter, the wear rates of Examples 1, 2 and 3 are lower than those of Comparative Examples 1 and 2, and their expected service lives are higher than those of Comparative Examples 1 and 2.

[0072] This shows that the main properties of medium chromium cast iron floating oil seals, such as wear resistance and service life, can reach or exceed those of high chromium cast iron and Ni-hard series high nickel cast iron, making it the main material for floating oil seal applications.

[0073] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A process for producing medium chromium cast iron floating oil seals by centrifugal casting, characterized in that: The following steps are involved: S1. The ingredients are prepared according to the standard requirements of medium chromium cast iron, and the prepared alloy raw materials are placed in a medium frequency furnace for smelting. After smelting, the castings are detected by a spectrometer and the composition of the molten iron is adjusted to be within the standard range of medium chromium cast iron. The weight percentage content of the elements in medium chromium cast iron is in the range of C2.8%-3.8%, Si1.0%-2.5%, Cr6.0%-12.0%, Mn0.2%-1.0%, Nb0.25%, Mo0.16%, Re0.21%, and the rest is Fe; S2, purify the molten iron according to the operating process, detect the temperature of the molten iron with a contact temperature measuring gun, control the temperature of the molten iron to 1480-1620°C, and then pour it out of the furnace; S3, using a centrifugal process method for casting, specifically: clean the impurities in the mold, the top mold mechanism falls back, the mold falls and closes, start the centrifugal device, scoop the molten iron with a crucible, and directly pour the specified volume of molten iron into the rotating mold cavity to form a casting mold. Under the action of centrifugal force, the molten iron quickly fills the mold outward from the pouring point, then the timer is started, and after the timing is completed, the centrifugal device is stopped. After the device stops steadily, the top mold mechanism is lifted, the mold is separated from the casting, and the medium chromium cast iron floating oil seal blank is obtained, and the impurities in the mold are cleaned to prepare for the next centrifugal casting; S4. The medium chrome cast iron floating oil seal blank is subjected to a process of rough machining, inner spherical grinding and sealing surface grinding to meet the corresponding size requirements and the surface roughness and flatness required for sealing performance, so as to obtain a medium chrome cast iron floating oil seal semi-finished product; the medium chrome cast iron floating oil seal semi-finished product is cleaned and inspected to obtain a medium chrome cast iron floating oil seal finished product.

2. The process for producing a medium chromium cast iron floating oil seal by centrifugal casting according to claim 1, characterized in that: The mold material is graphite.

3. The process for producing medium chromium cast iron floating oil seal by centrifugal casting according to claim 1, characterized in that: The mold is made of metal.

4. The process for producing a medium chromium cast iron floating oil seal by centrifugal casting according to claim 1, characterized in that: The Rockwell hardness of the medium chromium cast iron floating oil seal is HRc55-65.

5. The process for producing a medium chromium cast iron floating oil seal by centrifugal casting according to claim 1, characterized in that: The rotation speed of the mold in the centrifugal device is 300-1500rpm.

6. The process for producing a medium chromium cast iron floating oil seal by centrifugal casting according to claim 1, characterized in that: The centrifugation time of the centrifugal device is 20-180 seconds.

Citation Information

Patent Citations

  • Double-end centrifugal casting machine for floating oil seals of engineering machinery

    CN103056324A

  • High-chromium cast iron and casting method thereof

    CN105695854A

  • Casting device and casting method thereof

    CN108057864A

  • Floating seal ring for floating oil seal and preparation method of floating seal ring

    CN115700290A

  • High-wear-resistance medium-chromium cast iron fine-grain material as well as preparation method and application thereof

    CN115896605A