Foamed nickel-based positive electrode material, preparation method thereof and battery

By forming a sodium ferrous sulfate structure on the foamed nickel-based cathode material, the problem of poor conductivity of sodium-ion batteries is solved, the energy density and cycle life of the battery are improved, and the performance of efficient sodium-ion batteries is improved.

CN118389987BActive Publication Date: 2024-10-01JIANGSU PYLON BATTERY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410828015.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-01
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

Sodium-ion batteries suffer from low energy density and poor electrical conductivity, which limits their performance and applications.

Method used

Using foamed nickel-based cathode material, the nickel iron carbon nitrogen precursor is generated through the reaction of the nickel oxide layer and nickel ferricyanide, and reacts with sulfate ions and complexing agents under hydrothermal conditions to form foamed nickel composite sodium ferrous sulfate. structure, increasing the specific surface area and conductivity of the material.

Benefits of technology

It significantly improves the capacity and conductivity of the cathode material, improves the energy density and cycle life of sodium-ion batteries, and the nickel foam is self-supporting and suitable as a direct cathode sheet material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118389987B_ABST
    Figure CN118389987B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of battery materials, and discloses a foamed nickel-based positive electrode material, a preparation method thereof, and a battery. The preparation method of the foamed nickel-based positive electrode material comprises: oxidizing the foamed nickel to form a nickel oxide layer on its surface to obtain oxidized foamed nickel; mixing the oxidized foamed nickel with an acid solution of ferrocyanide to react the nickel oxide on the surface of the oxidized foamed nickel with ferrocyanide to generate nickel ferrocyanide to obtain foamed nickel-loaded nickel ferrocyanide; calcining the foamed nickel-loaded nickel ferrocyanide to obtain a nickel-iron-carbon-nitrogen precursor; hydrothermally reacting the nickel-iron-carbon-nitrogen precursor, sulfate ions, a complexing agent, and sodium ions, extracting the solid material after the reaction and calcining it to obtain a foamed nickel-based positive electrode material. The positive electrode material prepared by this method has an ultra-high specific surface area, good conductivity, and high capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a foamed nickel-based positive electrode material and a preparation method thereof and a battery. Background Art

[0002] Sodium ion batteries are batteries that use layered oxides (such as nickel iron manganese oxide and copper iron manganese oxide) materials, Prussian blue analogs (such as iron-based Prussian white, etc.), polyanions (such as sodium ferrous sulfate, sodium iron phosphate, etc.) as positive electrodes, and carbon materials (such as hard carbon, soft carbon) as negative electrodes. They mainly use esters and ethers as solvents. + Metal salts (such as sodium fluoride salts, sodium borate salts and perchlorates) electrolytes and various additives (such as film-forming, flame retardant and overcharge protection) form electrolytes. Although sodium-ion batteries have advantages such as good low-temperature performance, low cost, high safety and long cycle life, they still have serious problems such as low energy density and poor conductivity.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The purpose of the present invention is to provide a foamed nickel-based positive electrode material, a preparation method thereof and a battery. The positive electrode has an excellent three-dimensional structure, and is loaded with carbon and sodium ferrous sulfate for increasing conductivity, so that the positive electrode material has an ultra-high specific surface area, greatly improving the capacity of the positive electrode material, and stimulating the potential of polyanion materials for sodium ion batteries.

[0005] The present invention is achieved in that:

[0006] In a first aspect, the present invention provides a method for preparing a foamed nickel-based positive electrode material, comprising:

[0007] Oxidizing the nickel foam to form a nickel oxide layer on the surface of the nickel foam to obtain an oxidized nickel foam;

[0008] The oxidized nickel foam and the acid solution of ferrocyanide are mixed and reacted to make the nickel oxide on the surface of the oxidized nickel foam react with the ferrocyanide to generate nickel ferrocyanide, thereby obtaining nickel foam-loaded nickel ferrocyanide;

[0009] The nickel foam loaded nickel ferrocyanide is placed at 500-700° C. and calcined for 1-5 hours in a first inert atmosphere to obtain a nickel-iron-carbon-nitrogen precursor;

[0010] A nickel-iron-carbon-nitrogen precursor, sulfate ions, a complexing agent and sodium ions are subjected to a hydrothermal reaction to obtain a mixed slurry after the reaction is completed;

[0011] Extracting the solid material from the mixed slurry to obtain a foamed nickel composite sodium ferrous sulfate precursor;

[0012] The foamed nickel-composite sodium ferrous sulfate precursor is calcined at 300-500° C. in a second inert atmosphere for 4-8 hours to obtain a foamed nickel-based positive electrode material.

[0013] In an optional embodiment, the method of oxidizing the nickel foam includes:

[0014] The nickel foam is placed in an oxygen environment at 100-140°C for oxidation treatment for 0.5-1.5h.

[0015] In an optional embodiment, before the nickel foam is oxidized, the surface of the nickel foam is treated to remove the original uneven oxide layer on the surface of the nickel foam;

[0016] The method of removing the original uneven oxide layer on the surface of the nickel foam includes: washing the nickel foam with acetone and water in turn, and then placing it in an acid solution for reaction.

[0017] In an optional embodiment, the acid solution is selected from at least one of dilute sulfuric acid, dilute hydrochloric acid, citric acid and tartaric acid.

[0018] In an optional embodiment, the molar concentration of the acid solution is 0.5-1 mol / L, and the reaction time is 1-6 h.

[0019] In an optional embodiment, the preparation method provided by the present invention comprises at least one of the following features (1) to (14);

[0020] (1) The pH of the acid solution of ferrocyanide is 2 to 5;

[0021] (2) the ferrocyanide is at least one selected from the group consisting of potassium ferrocyanide, potassium ferrocyanide and sodium ferrocyanide;

[0022] (3) The first inert atmosphere is an argon atmosphere;

[0023] (4) The mixed reaction of the nickel oxide foam and the acid solution of ferrocyanide is carried out in a sealed container;

[0024] (5) The molar concentration of ferrocyanide in the acid solution of ferrocyanide is 0.1~0.7 mol / L;

[0025] (6) The mass ratio of the acid solution of ferrocyanide to the nickel oxide foam is 200-100:5;

[0026] (7) The complexing agent is citrate ion;

[0027] (8) The complexing agent is citrate ion, and the molar ratio of citrate ion to sodium ion is 1:5-10;

[0028] (9) The complexing agent is a citrate ion, and the citrate ion is provided by at least one of citric acid and a citrate salt;

[0029] (10) The sulfate ions for the hydrothermal reaction are provided by at least one of sulfuric acid and sulfate;

[0030] (11) The sodium ions for the hydrothermal reaction are provided by at least one sodium salt;

[0031] (12) The acid solution of ferrocyanide is a mixture of ferrocyanide and dilute acid, wherein the dilute acid is dilute sulfuric acid or dilute hydrochloric acid;

[0032] (13) The hydrothermal reaction temperature is 100~140℃, and the reaction time is 8~12h;

[0033] (14) The second inert atmosphere is an argon atmosphere, or a mixed atmosphere in which the volume ratio of argon to hydrogen is 1 to 2:1.

[0034] In an optional embodiment, the method of extracting the solid material from the mixed slurry includes:

[0035] The mixed slurry is subjected to solid-liquid separation, the obtained solid is washed with deionized water, and then dried to obtain a foamed nickel composite sodium ferrous sulfate precursor.

[0036] In an optional embodiment, the drying temperature is 80-120°C.

[0037] In a second aspect, the present invention provides a foamed nickel-based positive electrode material, which is prepared by the preparation method of any one of the aforementioned embodiments.

[0038] In a third aspect, the present invention provides a battery, wherein the positive electrode thereof is a foamed nickel-based positive electrode material as described in the foregoing embodiment.

[0039] The present invention has the following beneficial effects:

[0040] The preparation method provided in the embodiment of the present invention can prepare a foamed nickel-based positive electrode material. The positive electrode material uses foamed nickel as a matrix. The foamed nickel itself has a very high specific surface area. By using the method provided by the present invention, sodium ferrous sulfate particles are in-situ grown on the surface of the foamed nickel, and elemental N and C are loaded on the foamed nickel, so that a three-dimensional conductive structure with an ultra-high specific surface area can be obtained, which greatly improves the capacity of the positive electrode material; C is loaded on the foamed nickel to increase the conductivity of the material, and N in the positive electrode material can improve the conductivity and mechanical properties of the material; sodium ferrous sulfate is in-situ grown on the surface of the foamed nickel and has good connection stability with the foamed nickel matrix; the foamed nickel is self-supporting, so that the prepared positive electrode material can be directly used as a positive electrode sheet. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0042] Figure 1 This is a SEM image of the foamed nickel-based positive electrode material prepared in Example 1 of the present invention at a magnification of a;

[0043] Figure 2 This is a SEM image of the foamed nickel-based positive electrode material prepared in Example 1 of the present invention at a multiple of b that is greater than a multiple;

[0044] Figure 3 This is the XRD diagram of the surface particles of the foamed nickel-based positive electrode material obtained in Example 1 of the present invention after scraping off the surface particles. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0046] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0047] The following is a detailed description of the nickel-based positive electrode material and the preparation method thereof and the battery provided in the embodiments of the present invention.

[0048] An embodiment of the present invention provides a method for preparing a foamed nickel-based positive electrode material, comprising:

[0049] Oxidizing the nickel foam to form a nickel oxide layer on the surface of the nickel foam to obtain an oxidized nickel foam;

[0050] The oxidized nickel foam and the acid solution of ferrocyanide are mixed and reacted to make the nickel oxide on the surface of the oxidized nickel foam react with the ferrocyanide to generate nickel ferrocyanide, thereby obtaining nickel foam-loaded nickel ferrocyanide;

[0051] The nickel foam loaded nickel ferrocyanide is placed at 500-700° C. and calcined for 1-5 hours in a first inert atmosphere to obtain a nickel-iron-carbon-nitrogen precursor;

[0052] A nickel-iron-carbon-nitrogen precursor, sulfate ions, a complexing agent and sodium ions are subjected to a hydrothermal reaction to obtain a mixed slurry after the reaction is completed;

[0053] Extracting the solid material from the mixed slurry to obtain a foamed nickel composite sodium ferrous sulfate precursor;

[0054] The foamed nickel-composite sodium ferrous sulfate precursor is calcined at 300-500° C. in a second inert atmosphere for 4-8 hours to obtain a foamed nickel-based positive electrode material.

[0055] The preparation method provided in the embodiment of the present invention can prepare a foamed nickel-based positive electrode material. The positive electrode material uses foamed nickel as a matrix. The foamed nickel itself has a very high specific surface area. By using the method provided by the present invention, sodium ferrous sulfate particles are in-situ grown on the surface of the foamed nickel, and elemental N and C are loaded on the foamed nickel, so that a three-dimensional conductive structure with an ultra-high specific surface area can be obtained, which greatly improves the capacity of the positive electrode material; C is loaded on the foamed nickel to increase the conductivity of the material, and N in the positive electrode material can improve the conductivity and mechanical properties of the material; sodium ferrous sulfate is in-situ grown on the surface of the foamed nickel and has good connection stability with the foamed nickel matrix; the foamed nickel is self-supporting, so that the prepared positive electrode material can be directly used as a positive electrode sheet.

[0056] The preparation method is specifically as follows:

[0057] S1. Nickel foam pretreatment

[0058] Remove the original uneven oxide layer on the surface of nickel foam. The specific method is:

[0059] The nickel foam is washed with acetone and water successively, and then placed in an acid solution for reaction. After the reaction is completed, it is washed with deionized water for several times to obtain clean nickel foam.

[0060] Preferably, in order to fully remove the oxide layer on the surface of the nickel foam, the acid solution is selected from at least one of dilute sulfuric acid, dilute hydrochloric acid, citric acid and tartaric acid.

[0061] Preferably, the molar concentration of the acid solution is 0.5-1 mol / L (eg, 0.5 mol / L, 0.8 mol / L or 1 mol / L), and the reaction time is 1-6 h (eg, 1 h, 2 h, 4 h or 6 h).

[0062] The embodiment of the present invention uses commercial nickel foam as a raw material, which is cheap.

[0063] After the nickel foam surface is pretreated, there are no impurities and oxides on its surface, which can ensure that a uniform and dense nickel oxide layer is formed on the nickel foam surface during the subsequent pre-oxidation process, thereby ensuring that a positive electrode material with good electrochemical performance is obtained.

[0064] S2, Nickel Oxide Foam

[0065] The clean nickel foam is oxidized to form a uniform and dense nickel oxide layer on the surface of the nickel foam to obtain oxidized nickel foam.

[0066] Specifically, the method of oxidizing the nickel foam includes:

[0067] The nickel foam is placed in an oxygen environment at 100-140° C. (eg, 100° C., 120° C., or 140° C.) and oxidized for 0.5-1.5 h (eg, 0.5 h, 1 h, or 1.5 h).

[0068] S3. Preparation of nickel foam loaded with nickel ferrocyanide

[0069] The oxidized nickel foam and the acid solution of ferrocyanide are mixed and reacted, so that the nickel oxide on the surface of the oxidized nickel foam reacts with the ferrocyanide to generate nickel ferrocyanide, thereby obtaining the nickel foam-loaded nickel ferrocyanide.

[0070] The specific steps of this step are:

[0071] Weigh a certain amount of ferrocyanide and dissolve it in water, and use dilute acid to adjust the pH value to 3-4 to obtain an acid solution of ferrocyanide, which is then sealed for later use.

[0072] The oxidized nickel foam obtained in step S2 is placed in a sealed container of an acid solution of ferrocyanide and allowed to stand for about 1 hour, so that the surface of the nickel foam is evenly complexed with nickel ferrocyanide.

[0073] Optionally, the dilute acid is selected from at least one of dilute sulfuric acid and dilute hydrochloric acid.

[0074] Optionally, the molar concentration of ferrocyanide in the acid solution of ferrocyanide is 0.1-0.7 mol / L (e.g., 0.1 mol / L, 0.2 mol / L, 0.5 mol / L or 0.7 mol / L), preferably 0.25-0.5 mol / L (e.g., 0.25 mol / L, 0.3 mol / L or 0.5 mol / L).

[0075] Optionally, the dosage of the ferricyanide acid solution and the oxidized nickel foam is such that the oxidized nickel foam can be completely submerged in the ferricyanide acid solution.

[0076] Optionally, the ferrocyanide is selected from at least one of potassium ferrocyanide, potassium ferrocyanide and sodium ferrocyanide.

[0077] S4, first calcination

[0078] The nickel foam loaded with nickel ferrocyanide is placed in a tube furnace and calcined at 500-700° C. (eg, 500° C., 600° C. or 700° C.) in a first inert atmosphere for 1-5 h (eg, 1 h, 2 h, 3 h or 5 h) to obtain a nickel-iron-carbon-nitrogen precursor.

[0079] Inert gas high temperature carbonization cyanide can break some C-Fe bonds, thus obtaining some Fe 2+and iron element, in preparation for the subsequent hydrothermal reaction.

[0080] In this step, by setting a suitable calcination temperature and time, part of the cyanide can be left uncarbonized, so that part of the N element can remain in the final positive electrode material in the form of CN, thereby improving the electrochemical performance of the positive electrode material.

[0081] Optionally, the first inert atmosphere is an argon atmosphere.

[0082] S4, complexation to generate sodium ferrous sulfate

[0083] The sulfate ions, the complexing agent and the sodium ions are mixed and stirred evenly in the aqueous solution, and then placed in a hydrothermal reactor;

[0084] Add nickel-iron-carbon-nitrogen precursor to a hydrothermal reactor, set the reaction temperature to 100-140° C. (e.g., 100° C., 120° C., or 140° C.), and the reaction time to 8-12 h (e.g., 8 h, 10 h, or 12 h) to perform a hydrothermal reaction to generate a mixed slurry containing a foamed nickel composite sodium ferrous sulfate precursor.

[0085] Particles can be generated on the surface of nickel foam through hydrothermal reaction and complexing agent to ensure that the final cathode material has good electrochemical performance.

[0086] Optionally, the complexing agent is a citrate ion; further, the citrate ion is provided by at least one of citric acid and a citrate salt;

[0087] Optionally, the molar ratio of citrate ions to sodium ions is 1:5-10 (eg, 1:5, 1:8 or 1:10).

[0088] Optionally, the sulfate ions for the hydrothermal reaction are provided by at least one of sulfuric acid and sulfate;

[0089] Optionally, the sodium ions for the hydrothermal reaction are provided by at least one sodium salt.

[0090] Preferably, sulfate ions and sodium ions can come from the same compound, such as sodium sulfate; sulfate ions and sodium ions can come from different compounds, such as sulfuric acid and sodium hydroxide; citrate and sodium source can also come from the same compound, such as sodium citrate. In short, the material placed in the hydrothermal reactor only needs to provide sulfate ions, complexing agents and sodium ions. For example, this step can be to first prepare a certain amount of sodium sulfate solution, then add sodium citrate and stir evenly, and then place the obtained mixed solution in the hydrothermal reactor.

[0091] The amount of sulfur source and sodium source added can be fed in a stoichiometric ratio for generating sodium ferrous sulfate, and the sulfate ions, sodium ions and chelating agent in the hydrothermal reactor are in excess relative to the iron in the nickel-iron-carbon-nitrogen precursor, ensuring that the iron can react completely. Therefore, there is no excessive requirement for the feeding, even if the sulfate ions, sodium ions and chelating agent are in excess and there are surpluses after the reaction, the solution after the reaction product is extracted can be reused after the reaction is completed.

[0092] S5. Extraction of foam nickel composite sodium ferrous sulfate precursor

[0093] The mixed slurry obtained in step S4 is subjected to solid-liquid separation, and the obtained solid is washed with pure water, and then placed in an oven at 80-120° C. (eg, 80° C., 100° C. or 120° C.) for drying to obtain a foamed nickel composite sodium ferrous sulfate precursor.

[0094] S6. Second calcination

[0095] The nickel foam composite sodium ferrous sulfate precursor is placed in a tubular furnace, a second inert gas is introduced, the temperature is set to 300-500° C. (e.g., 300° C., 400° C., or 500° C.), and calcined for 4-8 hours (e.g., 4 hours, 6 hours, or 8 hours) to obtain a nickel foam-based positive electrode material loaded with N, C, and sodium ferrous sulfate.

[0096] It should be noted that the calcination temperature in this step should be within the above range. If the temperature is too high, the cyanide groups in the material will be completely carbonized, causing all N elements to be converted into N2 and escape. If the temperature is too low, the crystallinity of sodium ferrous sulfate will be low.

[0097] The foamed nickel-based positive electrode material loaded with N, C and sodium ferrous sulfate provided in the embodiment of the present invention is prepared by the preparation method provided in the embodiment of the present invention. The positive electrode has the characteristics of high capacity and long cycle life.

[0098] The positive electrode of the battery provided by the embodiment of the present invention is the foamed nickel-based positive electrode loaded with N, C and sodium ferrous sulfate provided by the embodiment of the present invention.

[0099] Specifically, for example, the foamed nickel-based positive electrode material loaded with N, C and sodium ferrous sulfate provided in the embodiment of the present invention can be used as the positive electrode, hard carbon can be used as the negative electrode, an organic electrolyte system and a PP separator can be used, and the stacking can be prepared as a sodium ion soft-pack battery.

[0100] The present invention is further described below in conjunction with a number of embodiments and comparative examples.

[0101] Example 1

[0102] The specific surface area is 100m 2 / g of nickel foam was washed with acetone and water successively, and then placed in a dilute hydrochloric acid solution with a mass concentration of 1 mol / L to react for 1 hour. After the reaction was completed, it was washed with deionized water for several times to obtain clean nickel foam;

[0103] The clean nickel foam is placed in an oxygen environment at 120°C for oxidation treatment for 1 hour to form a uniform and dense nickel oxide layer on the surface of the nickel foam;

[0104] Weigh 0.1 mol of potassium ferrocyanide and dissolve it in 200 ml of water. Use dilute sulfuric acid to adjust the pH value of the solution to 3.5 to obtain a potassium ferrocyanide acid solution with a potassium ferrocyanide molar concentration of 0.5 mol / L. Seal it for later use.

[0105] 5 g of nickel foam oxide was placed in a sealed container containing an acid solution of ferrocyanide and allowed to stand for 1 hour to obtain nickel foam loaded with nickel ferrocyanide;

[0106] The nickel foam loaded with nickel ferrocyanide was placed in a tube furnace and calcined at 600°C in an argon environment for 1 h to obtain a nickel-iron-carbon-nitrogen precursor;

[0107] Prepare 200 ml of 1 mol / L sodium sulfate solution, then add 0.04 mol of sodium citrate to the sodium sulfate solution and stir evenly, then place the obtained mixed solution in a hydrothermal reactor;

[0108] Adding nickel-iron-carbon-nitrogen precursor into a hydrothermal reactor, setting the reaction temperature to 120° C. and the reaction time to 10 h for hydrothermal reaction, to generate a mixed slurry containing a foamed nickel composite sodium ferrous sulfate precursor;

[0109] The mixed slurry is subjected to solid-liquid separation, and the obtained solid is washed with pure water for multiple times and then dried in an oven at 100° C. to obtain a foamed nickel composite sodium ferrous sulfate precursor;

[0110] The foamed nickel composite sodium ferrous sulfate precursor was placed in a tube furnace, a second inert gas was introduced, the temperature was set to 400°C, and calcined for 6 hours to obtain a foamed nickel-based positive electrode material. The SEM image of the foamed nickel-based positive electrode material was taken as shown in FIG. Figure 1 and Figure 2 As shown in the figure, it can be seen that tiny particles grow on the three-dimensional skeleton of the nickel foam; the particles on the surface of the nickel foam-based positive electrode material are scraped off and the XRD pattern is measured as follows Figure 3 As shown in the figure, it can be seen that the main component of these particles is sodium ferrous sulfate.

[0111] Example 2

[0112] The specific surface area is 100m 2 / g nickel foam was washed with acetone and water successively, and then placed in a dilute hydrochloric acid solution with a mass concentration of 1 mol / L to react for 1 hour. After the reaction was completed, it was washed with deionized water for several times to obtain clean nickel foam;

[0113] The clean nickel foam was placed in an oxygen environment at 100°C for 1.5 hours to form a uniform and dense nickel oxide layer on the surface of the nickel foam.

[0114] Weigh 0.05 mol of potassium ferrocyanide and dissolve it in 200 ml of water. Use dilute sulfuric acid to adjust the pH value of the solution to 4 to obtain a potassium ferrocyanide acid solution with a potassium ferrocyanide molar concentration of 0.25 mol / L. Seal it for later use.

[0115] 5 g of nickel oxide foam was placed in a sealed container containing potassium ferrocyanide acid solution and allowed to stand for 1 hour to obtain nickel foam loaded with nickel ferrocyanide;

[0116] The nickel foam loaded with nickel ferrocyanide was placed in a tube furnace and calcined at 500°C in an argon environment for 1 h to obtain a nickel-iron-carbon-nitrogen precursor;

[0117] Prepare 200 ml of 0.5 mol / L sodium sulfate solution, then add 0.02 mol of sodium citrate to the sodium sulfate solution and stir evenly, then place the obtained mixed solution in a hydrothermal reactor;

[0118] Adding nickel-iron-carbon-nitrogen precursor into a hydrothermal reactor, setting the reaction temperature to 100° C. and the reaction time to 12 h for hydrothermal reaction, to generate a mixed slurry containing a foamed nickel-composite sodium ferrous sulfate precursor;

[0119] The mixed slurry is subjected to solid-liquid separation, and the obtained solid is washed with pure water for multiple times and then dried in an oven at 100° C. to obtain a foamed nickel composite sodium ferrous sulfate precursor;

[0120] The nickel foam composite sodium ferrous sulfate precursor was placed in a tubular furnace, a second inert gas was introduced, the temperature was set to 300° C., and calcined for 8 hours to obtain a nickel foam-based positive electrode material.

[0121] Example 3

[0122] The specific surface area is 100m 2 / g nickel foam was washed with acetone and water successively, and then placed in a dilute hydrochloric acid solution with a mass concentration of 1 mol / L to react for 1 hour. After the reaction was completed, it was washed with deionized water for several times to obtain clean nickel foam;

[0123] The clean nickel foam was placed in an oxygen environment at 140°C for 0.5 h to form a uniform and dense nickel oxide layer on the surface of the nickel foam.

[0124] Weigh 0.1 mol of potassium ferrocyanide and dissolve it in 200 ml of water. Use dilute sulfuric acid to adjust the pH value of the solution to 3 to obtain a potassium ferrocyanide acid solution with a potassium ferrocyanide molar concentration of 0.5 mol / L. Seal it for later use.

[0125] 5 g of oxidized nickel foam was placed in a sealed container containing an acid solution of ferrocyanide and allowed to stand for 1 hour to obtain nickel foam loaded with nickel ferrocyanide;

[0126] The nickel foam loaded with nickel ferrocyanide was placed in a tube furnace and calcined at 700°C in an argon environment for 1 h to obtain a nickel-iron-carbon-nitrogen precursor;

[0127] Prepare 200 ml of 1 mol / L sodium sulfate solution, then add 0.04 mol of sodium citrate to the sodium sulfate solution and stir evenly, then place the obtained mixed solution in a hydrothermal reactor;

[0128] Adding nickel-iron-carbon-nitrogen precursor into a hydrothermal reactor, setting the reaction temperature to 140° C. and the reaction time to 8 h for hydrothermal reaction, to generate a mixed slurry containing a foamed nickel composite sodium ferrous sulfate precursor;

[0129] The mixed slurry is subjected to solid-liquid separation, and the obtained solid is washed with pure water for multiple times and then dried in an oven at 100° C. to obtain a foamed nickel composite sodium ferrous sulfate precursor;

[0130] The nickel foam composite sodium ferrous sulfate precursor was placed in a tubular furnace, argon gas was introduced, the temperature was set to 500°C, and calcined for 4 hours to obtain a nickel foam-based positive electrode loaded with N, C and sodium ferrous sulfate.

[0131] Comparative Example 1

[0132] This comparative example is basically the same as Example 2, except that the nickel foam loaded with nickel ferrocyanide is placed in a tubular furnace and calcined at 300° C. in an argon environment for 1 h to obtain a nickel-iron-carbon-nitrogen precursor.

[0133] Comparative Example 2

[0134] This comparative example is basically the same as Example 3, except that the nickel foam loaded with nickel ferrocyanide is placed in a tubular furnace and calcined at 800° C. in an argon environment for 1 h to obtain a nickel-iron-carbon-nitrogen precursor.

[0135] Comparative Example 3

[0136] This comparative example is basically the same as Example 2, except that the foamed nickel composite sodium ferrous sulfate precursor is placed in a tube furnace and calcined at 250° C. in an argon environment for 4 hours to obtain a foamed nickel-based positive electrode loaded with N, C and sodium ferrous sulfate.

[0137] Comparative Example 4

[0138] This comparative example is basically the same as Example 3, except that the foamed nickel composite sodium ferrous sulfate precursor is placed in a tube furnace and calcined at 700° C. in an argon environment for 4 hours to obtain a foamed nickel-based positive electrode loaded with N, C and sodium ferrous sulfate.

[0139] Comparative Example 5

[0140] Ordinary sodium ferrous sulfate is used as the active material, and the positive electrode sheet is prepared by coating with an oil-based formula, specifically:

[0141] N-methylpyrrolidone was used as solvent, the solid matter composition was sodium ferrous sulfate, PVDF, SP and PVP, the mass ratio of sodium ferrous sulfate, PVDF, SP and PVP was (100:7:10:3), and the positive electrode sheet was prepared by coating aluminum foil.

[0142] Experimental example

[0143] The foamed nickel-based positive electrode material prepared in the above-mentioned embodiments and comparative examples was coated with an oil-based formula to prepare a positive electrode sheet, and the hard carbon water-based formula was coated to prepare a negative electrode sheet. A polypropylene separator was selected as the separator, and 1M sodium salt + ester solvent (EC / DMC) was selected as the electrolyte to prepare a laminated 5Ah soft-pack battery.

[0144] Each embodiment and comparative example was tested for 0.1C / 0.1C charge / discharge capacity, first coulomb efficiency, capacity retention rate at 5C rate, capacity retention rate after 100 cycles of 0.1C / 0.1C charge / discharge, gas production after 100 cycles of 0.1C / 0.1C charge / discharge, and capacity retention rate after 100 cycles of 0.5C / 1C high temperature cycles. The test results are recorded in Table 1.

[0145] Table 1 Electrochemical properties of the batteries prepared in the examples and comparative examples

[0146]

[0147] It can be seen from Table 1 that after the positive electrodes prepared in various embodiments of the present invention are assembled into batteries, compared with Comparative Example 5, the contact area between the electrode and the electrolyte is enhanced, the energy density and power density are improved, and the nickel foam improves the conductivity and mechanical strength of the electrode, which is beneficial to the recycling of the battery. This shows that the positive electrode materials prepared in the embodiments of the present invention have excellent electrochemical properties; the specific surface area of ​​the positive electrode materials prepared in various embodiments is greatly improved compared with the nickel foam before preparation.

[0148] Comparing Examples 2 and 3 with Comparative Examples 1 and 2, respectively, the conductivity of Comparative Example 1 is poor, and the active material of Comparative Example 2 is less, indicating that the first calcination temperature should be within 500-700°C. Calcination at too high or too low a temperature will reduce the electrochemical performance of the obtained positive electrode material.

[0149] Comparing Examples 2 and 3 with Comparative Examples 3 and 4 respectively, the active material crystallinity of Comparative Example 2 is poor, and the conductivity and mechanical properties of Comparative Example 3 are poor, indicating that the second calcination temperature should be within 300-500°C. Calcination at too high or too low a temperature will reduce the electrochemical performance of the obtained positive electrode.

[0150] In summary, the preparation method provided in the embodiment of the present invention can prepare a nickel foam-based positive electrode material, which takes nickel foam as a matrix. The nickel foam itself has a very high specific surface area. By the method provided by the present invention, sodium ferrous sulfate particles are in situ grown on the surface of the nickel foam, and elemental N and C are loaded on the nickel foam, so that a three-dimensional conductive structure with an ultra-high specific surface area can be obtained, which greatly improves the capacity of the positive electrode material; C loading on the nickel foam has the effect of increasing the conductivity of the material, and N in the positive electrode material can play a role in improving the conductivity and mechanical properties of the material; sodium ferrous sulfate is in situ grown on the surface of the nickel foam and has a good connection stability with the nickel foam matrix; the nickel foam has self-supporting properties, so that the prepared positive electrode material can be directly used as a positive electrode sheet.

[0151] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a foamed nickel-based positive electrode material, characterized in that: include: Oxidizing the nickel foam to form a nickel oxide layer on the surface of the nickel foam to obtain an oxidized nickel foam; Mixing the oxidized nickel foam and an acid solution of ferrocyanide to react, so that the nickel oxide on the surface of the oxidized nickel foam reacts with the ferrocyanide to generate nickel ferrocyanide, thereby obtaining nickel foam-loaded nickel ferrocyanide; The nickel foam loaded with nickel ferrocyanide is placed at 500-700° C. and calcined for 1-5 hours in a first inert atmosphere to obtain a nickel-iron-carbon-nitrogen precursor; Allowing the nickel-iron-carbon-nitrogen precursor, sulfate ions, a complexing agent and sodium ions to undergo a hydrothermal reaction, and obtaining a mixed slurry after the reaction is completed; Extracting the solid material from the mixed slurry to obtain a foamed nickel composite sodium ferrous sulfate precursor; The foamed nickel composite sodium ferrous sulfate precursor is calcined at 300-500° C. in a second inert atmosphere for 4-8 hours to obtain a foamed nickel-based positive electrode material.

2. The preparation method according to claim 1, characterized in that: The methods for oxidizing nickel foam include: The nickel foam is placed in an oxygen environment at 100-140°C for oxidation treatment for 0.5-1.5h.

3. The preparation method according to claim 1, characterized in that: Before the nickel foam is oxidized, the surface of the nickel foam is treated to remove the original uneven oxide layer on the surface of the nickel foam; The method of removing the original uneven oxide layer on the surface of the nickel foam includes: washing the nickel foam with acetone and water in turn, and then placing it in an acid solution for reaction.

4. The preparation method according to claim 3, characterized in that: The acid solution is selected from at least one of dilute sulfuric acid, dilute hydrochloric acid, citric acid and tartaric acid.

5. The preparation method according to claim 3, characterized in that: The molar concentration of the acid solution is 0.5-1 mol / L, and the reaction time is 1-6 h.

6. The preparation method according to claim 1, characterized in that: The invention comprises at least one of the following features (1) to (12); (1) The pH of the acid solution of ferrocyanide is 2 to 5; (2) The ferrocyanide is at least one selected from potassium ferrocyanide, potassium ferrocyanide and sodium ferrocyanide; (3) The first inert atmosphere is an argon atmosphere; (4) The mixed reaction of the nickel oxide foam and the acid solution of ferrocyanide is carried out in a sealed container; (5) The molar concentration of ferrocyanide in the acid solution of ferrocyanide is 0.1-0.7 mol / L; (6) The mass ratio of the acidic solution of ferrocyanide to the oxidized nickel foam is 200-100:5; (7) The complexing agent is a citrate ion; (8) The sulfate ions for the hydrothermal reaction are provided by at least one of sulfuric acid and sulfate; (9) The sodium ions for the hydrothermal reaction are provided by at least one sodium salt; (10) The acid solution of ferrocyanide is a mixture of ferrocyanide and dilute acid, wherein the dilute acid is dilute sulfuric acid or dilute hydrochloric acid; (11) The hydrothermal reaction temperature is 100~140℃ and the reaction time is 8~12h; (12) The second inert atmosphere is an argon atmosphere, or a mixed atmosphere in which the volume ratio of argon to hydrogen is 1 to 2:

1.

7. The preparation method according to claim 1, characterized in that: The complexing agent is a citrate ion, and the citrate ion is provided by at least one of citric acid and citrate.

8. The preparation method according to claim 1, characterized in that: The complexing agent is citrate ion, and the molar ratio of the citrate ion to the sodium ion is 1:5-10.

9. The preparation method according to claim 1, characterized in that: The method of extracting the solid material from the mixed slurry includes: The mixed slurry is subjected to solid-liquid separation, the obtained solid is washed with deionized water, and then dried to obtain the foamed nickel composite sodium ferrous sulfate precursor.

10. The preparation method according to claim 9, characterized in that: The drying temperature is 80~120℃.

11. A foamed nickel-based positive electrode material, characterized in that: The method is prepared according to any one of claims 1 to 10.

12. A battery, characterized in that: The positive electrode is the foamed nickel-based positive electrode material as claimed in claim 11.

Citation Information

Patent Citations

  • Self-supporting positive electrode and preparation method and application thereof

    CN116435467A

  • Hollow spherical sodium ferrous sulfate / carbon composite positive electrode material, preparation method and sodium ion battery prepared from hollow spherical sodium ferrous sulfate / carbon composite positive electrode material

    CN117727883A

  • Element-doped dual-carbon modified sodium ferrous sulfate positive electrode material and preparation method and application thereof

    CN118099392A

  • Sodium ferric sulfate positive electrode material, preparation method thereof, positive electrode plate and sodium ion battery

    CN118198303A

  • Micron-sized porous sodium ferrous sulfate / carbon composite positive electrode material and sodium ion battery or sodium battery prepared from same

    WO2023087485A1