Sealing material analysis method
The melting temperature and performance of the oxide composition are analyzed through thermochemical calculations and various testing methods, which solves the problem of analyzing sealing materials in high-temperature environments, optimizes the sealing performance of solid oxide fuel cells, and reduces energy consumption and cost.
Patent Information
- Application Number
- CN202410852357.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-28
AI Technical Summary
It is difficult to analyze sealing materials, especially in evaluating their stability and molten state properties in high-temperature environments, which makes it difficult to meet the sealing operation requirements of solid oxide fuel cells.
Thermochemical calculation software is used to calculate the melting temperature of the oxide composition, and melting, water quenching, and ball milling are performed to obtain glass powder, which is tested and analyzed through X-ray photoelectron spectroscopy, Raman spectroscopy, and differential scanning calorimetry. Relationship between oxygen structure and temperature properties.
Through process processing and test analysis, the relationship between the oxygen structure and temperature performance of the sealing material was clarified, solving the difficulty of analysis, reducing energy consumption, and achieving low-cost material performance optimization.
Smart Images

Figure CN118392919B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of material technology, and in particular to a sealing material analysis method. Background Art
[0002] Solid Oxide Fuel Cell (SOFC) is a new type of power generation device. Due to its advantages of high efficiency, pollution-free, all-solid-state structure and wide adaptability to a variety of fuel gases, it has broad application prospects in large-scale power stations, distributed power supply systems, military and other fields. Fuel gas and air pass through the two sides of the SOFC stack respectively. It is necessary to separate the fuel gas and air at the edge of the battery through sealing materials under high temperature environment. Long time (such as 40000h), medium and high temperature (such as 600℃ to 800℃), strong airflow impact and frequent hot and cold cycles (such as thousands of times) are strict tests for sealing materials. In order to meet the sealing operation requirements of solid oxide fuel cell SOFC, the sealing glass material must have suitable high temperature performance and stability.
[0003] The preparation process of sealing materials involves a high-temperature molten state, which has poor stability and is prone to element volatilization. It is difficult to evaluate the properties of glass only from a thermodynamic perspective. At present, there is a problem of difficulty in analyzing sealing materials.
[0004] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention
[0005] The purpose of the present disclosure is to provide a sealing material analysis method, thereby overcoming the problem of difficulty in sealing material analysis at least to a certain extent.
[0006] The present disclosure provides a sealing material analysis method, comprising: calculating the melting temperature of each oxide composition in a plurality of oxide compositions using thermochemical calculation software, wherein the oxide contents contained in the oxide compositions are not completely the same; melting the oxide compositions at a target temperature to obtain a glass liquid; wherein the target temperature is higher than the melting temperature of the oxide compositions; quenching the glass liquid with water and drying it to obtain glass slag; ball-milling the glass slag to obtain glass powder; testing and analyzing the glass powder corresponding to each oxide composition to obtain the relationship between the oxygen structure and the temperature performance of the sealing material.
[0007] Alternatively, the oxide composition comprises 20 wt % to 40 wt % SiO 2 , 30 wt % to 60 wt % B 2 O 3 , 10 wt % to 30 wt % SrO, 5 wt % to 20 wt % MgO, and 1 wt % to 5 wt % Na 2 O.
[0008] Optionally, the sealing material analysis method further includes: obtaining a plurality of oxides in proportion; and putting the plurality of oxides into a mixer for mechanical mixing to obtain an oxide composition.
[0009] Optionally, the temperature difference between the target temperature and the melting temperature of the oxide composition is greater than 100°C to 200°C.
[0010] Optionally, melting the oxide composition at a target temperature to obtain molten glass includes: melting the oxide composition at the target temperature for 2 hours to 6 hours using an alumina crucible or a magnesia crucible to obtain molten glass.
[0011] Optionally, the glass liquid is subjected to water quenching treatment and then dried to obtain glass slag, including: using deionized water to quench the glass liquid and then drying to obtain glass slag.
[0012] Optionally, the ball milling treatment uses alumina balls and alumina ball mill jars, the diameters of the alumina balls include 2mm, 5mm and 8mm, the ball-to-material ratio is 3:1 to 5:1, the ball milling rotation speed is 200r / min to 400r / min, and the ball milling time is 4h to 10h.
[0013] Optionally, the glass powder corresponding to each oxide composition is tested and analyzed to obtain the relationship between the oxygen structure and temperature performance of the sealing material, including: performing X-ray photoelectron spectroscopy testing on the glass powder corresponding to each oxide composition to obtain the oxygen structure of the sealing material; performing differential scanning calorimetry testing on the glass powder corresponding to each oxide composition to obtain the temperature performance of the sealing material; wherein the temperature performance includes glass transition temperature and / or glass softening temperature; and performing data fitting using the oxygen structure and temperature performance of each sealing material to obtain the relationship between the oxygen structure and temperature performance of the sealing material.
[0014] Optionally, the sealing material analysis method further includes: testing and analyzing the glass powder corresponding to each oxide composition to obtain the relationship between the network structure composition and temperature performance of the sealing material.
[0015] Optionally, the glass powder corresponding to each oxide composition is tested and analyzed to obtain the relationship between the network structure composition and the temperature performance of the sealing material, including: performing Raman spectroscopy testing on the glass powder corresponding to each oxide composition to obtain the network structure composition of the sealing material; performing differential scanning calorimetry testing on the glass powder corresponding to each oxide composition to obtain the temperature performance of the sealing material; wherein the temperature performance includes glass transition temperature and / or glass softening temperature; and performing data fitting using the network structure composition and temperature performance of each sealing material to obtain the relationship between the network structure composition and the temperature performance of the sealing material.
[0016] Through the sealing material analysis method of the embodiment of the present disclosure, on the one hand, through process treatment and test analysis, the relationship between the oxygen structure and temperature performance of the sealing material can be obtained, which at least solves the problem of the difficulty of sealing material analysis to a certain extent. Based on this, the temperature performance of the sealing material can be further designed and regulated through the oxygen structure to meet the application requirements of solid oxide fuel cell sealing materials; on the other hand, the present disclosure adopts processes such as melting, water quenching, and ball milling, which has low energy consumption and avoids energy waste; on the other hand, the present disclosure obtains the relationship between oxygen structure and temperature performance through a limited number of processing processes, which is easy to implement and low cost.
[0017] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.
[0019] Figure 1 The flowchart of the sealing material analysis method according to the exemplary embodiment of the present disclosure is schematically shown.
[0020] Figure 2 The software interface diagram for calculating the melting start temperature of Example 1 of the present disclosure is shown.
[0021] Figure 3 The software interface diagram for calculating the complete melting temperature of Example 1 of the present disclosure is shown.
[0022] Figure 4 A schematic diagram showing the fitting results of the X-ray photoelectron spectrum of Example 1 of the present disclosure is shown.
[0023] Figure 5A schematic diagram showing the fitting results of the Raman spectrum of Example 1 of the present disclosure is shown.
[0024] Figure 6 A schematic diagram showing a differential scanning calorimetry (DSC) curve of Example 1 of the present disclosure.
[0025] Figure 7 The software interface diagram for calculating the melting start temperature of Example 2 of the present disclosure is shown.
[0026] Figure 8 The software interface diagram for calculating the complete melting temperature of Example 2 of the present disclosure is shown.
[0027] Fig. 9 A schematic diagram showing the fitting results of the X-ray photoelectron spectrum of Example 2 of the present disclosure is shown.
[0028] Fig.10 A schematic diagram showing the fitting results of the Raman spectrum of Example 2 of the present disclosure is shown.
[0029] Fig.11 A schematic diagram showing the DSC curve of Example 2 of the present disclosure is shown.
[0030] Fig.12 A schematic diagram showing the relationship between the fitted oxygen structure and temperature performance according to an embodiment of the present disclosure.
[0031] Fig.13 A schematic diagram showing the relationship between the fitted network structure composition and temperature performance of an embodiment of the present disclosure is shown. DETAILED DESCRIPTION
[0032] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, processes, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.
[0033] In addition, the accompanying drawings are only schematic illustrations of the present disclosure and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated descriptions will be omitted. The flowcharts shown in the accompanying drawings are only exemplary illustrations and do not necessarily include all the steps. For example, some steps can also be decomposed, while some steps can be combined or partially combined, so the actual execution order may change according to actual conditions. In addition, all the terms "first", "second", "third", etc. below are only for the purpose of distinction and should not be used as limitations of the present disclosure.
[0034] The sealing material mentioned in the embodiment of the present disclosure can also be called a sealing glass material.
[0035] In view of the current difficulties in evaluating the properties of sealing materials from a thermodynamic perspective, the present disclosure at least provides a solution for analyzing the relationship between the oxygen structure and the temperature performance of the sealing material.
[0036] Oxygen structure is a key parameter for the sealing and stability of the sealing glass system. In the glass structure, taking silicate as an example, [SiO4] tetrahedron is the basic structural unit of all silicates and aluminosilicates. When other cations are added, they will break the Si-O bond and replace it with MO (M is a cation) bond. The transition temperature Tg and softening temperature Ts of the glass are important indicators for evaluating the performance of sealing glass materials. The Tg of the sealing glass should be slightly lower than the operating temperature, which is conducive to releasing the thermal stress between the glass and adjacent components and repairing cracks caused by stress. The type and content of oxygen structure in the glass network will significantly affect the Tg and Ts of the glass. The increase of non-bridging oxygen and free oxygen will weaken the connectivity of the glass network structure and reduce Si 4+ Tetrahedral coordination leads to a decrease in the strength of the internal structure of the glass, thereby reducing Tg and Ts. Therefore, the oxygen structure is related to the network structure composition, and optimizing the type and content of oxygen structure in the system is an effective way to adjust the high temperature performance of glass.
[0037] Figure 1 The flowchart of the sealing material analysis method according to an exemplary embodiment of the present disclosure is schematically shown. Figure 1 The sealing material analysis method of the embodiment of the present disclosure may include the following steps:
[0038] S10. Calculating the melting temperature of each oxide composition in a plurality of oxide compositions using thermochemical calculation software, wherein the content of oxides contained in each oxide composition is not completely the same.
[0039] In an exemplary embodiment of the present disclosure, the oxide composition may include 20 wt % to 40 wt % of SiO2, 30 wt % to 60 wt % of B2O3, 10 wt % to 30 wt % of SrO, 5 wt % to 20 wt % of MgO, and 1 wt % to 5 wt % of Na2O. It should be understood that the above oxides and contents are only exemplary. For example, the oxide composition described in the present disclosure may also include oxides such as Al2O3.
[0040] The present disclosure does not limit the number of oxide compositions. It is understood that the more oxide compositions are selected, the more accurate the final analysis results are, but the time, material, process, test and other costs are higher; the fewer oxide compositions are selected, the less time, material, process, test and other costs are, but the accuracy of the final analysis results may decrease.
[0041] According to some embodiments of the present disclosure, for each oxide composition to which the present disclosure is applied, the oxide types contained in them may be the same, that is, each oxide composition may contain SiO2, B2O3, SrO, MgO and Na2O. However, the contents of the oxides contained in the oxide compositions are not completely the same. It is understood that not completely the same includes completely different and only partially the same. For example, the plurality of oxide compositions include a first oxide composition, a second oxide composition, and a third oxide composition, wherein the first oxide composition comprises 20 wt% SiO2, 50 wt% B2O3, 15 wt% SrO, 10 wt% MgO, and 5 wt% Na2O, the second oxide composition comprises 25 wt% SiO2, 45 wt% B2O3, 15 wt% SrO, 10 wt% MgO, and 5 wt% Na2O, and the third oxide composition comprises 40 wt% SiO2, 30 wt% B2O3, 10 wt% SrO, 19 wt% MgO, and 1 wt% Na2O. It should be understood that the above specific contents are only exemplary, however, after experimental determination, the content range of each oxide is as described above and will not be repeated.
[0042] According to other embodiments of the present disclosure, for each oxide composition to which the present disclosure is applied, the types of oxides contained in them may not be completely the same. For example, the plurality of oxide compositions include an oxide composition A and an oxide composition B, wherein the oxide composition A includes SiO2, B2O3, SrO, MgO and Na2O, and the oxide composition B includes four oxides of SiO2, B2O3, SrO, MgO and Na2O. In addition, in these embodiments, the concept of the oxide contents being completely different is as described above and will not be repeated.
[0043] In an exemplary embodiment of the present disclosure, the melting temperature of each oxide composition in the plurality of oxide compositions can be calculated using thermochemical calculation software. Specifically, FactSage thermodynamic software can be used, the FToxid database can be selected, the total mass of the oxide composition is calculated as 100 g, for example, in the Equilib module, after the components are input, Slag-liq is selected as the base phase, and the melting temperature of each oxide composition is calculated.
[0044] S12. Melting the oxide composition at a target temperature to obtain molten glass; wherein the target temperature is higher than the melting temperature of the oxide composition.
[0045] For the actual process, it is necessary to first obtain each oxide composition. For the process of obtaining an oxide composition, first, multiple oxides can be obtained in proportion, and the proportion can correspond to the above-mentioned oxide content. The present disclosure does not limit the specific value selected from the content range. Next, these multiple oxides can be put into a mixer for mechanical mixing to obtain an oxide composition. It is understandable that for the acquisition of multiple oxide compositions, the above-mentioned acquisition operation needs to be performed multiple times.
[0046] The process is described by taking any one of the multiple oxide compositions as an example. After obtaining the oxide composition, the oxide composition can be melted at a target temperature to obtain a glass liquid. The glass liquid is a clear glass liquid.
[0047] The target temperature is configured to be higher than the melting temperature of the oxide composition calculated in step S10. Specifically, the target temperature may be configured to have a temperature difference greater than 100°C to 200°C from the melting temperature.
[0048] In addition, an alumina crucible or a magnesia crucible may be used to implement the above melting process, and the melting time may be configured to be 2 hours to 6 hours. It is understandable that the melting time may vary depending on the target temperature.
[0049] S14. The glass liquid is subjected to water quenching and drying to obtain glass slag.
[0050] In an exemplary embodiment of the present disclosure, the glass liquid may be quenched with deionized water to avoid the introduction of impurities. After the glass liquid is quenched and dried, glass slag may be obtained.
[0051] S16. Ball milling the glass slag to obtain glass powder.
[0052] In an exemplary embodiment of the present disclosure, the ball milling process can use alumina balls and alumina ball milling jars. The diameters of the alumina balls include 2 mm, 5 mm and 8 mm. The ball-to-material ratio is 3:1 to 5:1, and specifically, the ball-to-material ratio can be configured to be 4:1. The rotation speed of the ball milling process is 200 r / min to 400 r / min, and the ball milling time is 4 h to 10 h.
[0053] After ball milling, micron-sized glass powder can be obtained by sieving.
[0054] S18. Testing and analyzing the glass powder corresponding to each oxide composition to obtain the relationship between the oxygen structure and temperature performance of the sealing material.
[0055] It is understandable that for practical application of sealing materials, the glass powder may need to be further processed, such as through casting, lamination, etc. However, for analysis of sealing materials, the glass powder can be directly used.
[0056] According to some embodiments of the present disclosure, on the one hand, the glass powder corresponding to each oxide composition can be subjected to an X-ray photoelectron spectroscopy test to obtain the oxygen structure of the sealing material. The parameters used in the X-ray photoelectron spectroscopy test include: the excitation source uses Al Kα rays (hv = 1486.6eV), the working voltage is 14.6 KV, the filament current is 13.5 mA, and 20 cycles of signal accumulation are performed. The test passing energy is 20eV, the step size is 0.1eV, and the charge correction is performed using the C 1s = 284.8eV binding energy as the energy standard. AVANTAGE software is then used for fitting analysis to obtain the oxygen structure composition.
[0057] On the other hand, the glass powder corresponding to each oxide composition can be subjected to a differential scanning calorimetry test to obtain the temperature performance of the sealing material. The temperature performance in the disclosed embodiment may include a glass transition temperature and / or a glass softening temperature. Among them, the parameters of the differential scanning calorimetry test include: a heating rate of 10°C / min, and a heating range of room temperature to 1200°C.
[0058] Next, the oxygen structure and temperature performance of each sealing material obtained through multiple process tests can be used for data fitting to obtain the relationship between the oxygen structure and temperature performance of the sealing material. Specifically, Origin software can be used to draw a graph to obtain a visual result.
[0059] According to other embodiments of the present disclosure, the glass powder corresponding to each oxide composition may be tested and analyzed to obtain the relationship between the network structure composition and temperature performance of the sealing material.
[0060] On the one hand, the glass powder corresponding to each oxide composition can be tested by Raman spectroscopy to obtain the network structure of the sealing material. The parameters of the Raman spectroscopy test include: the wavelength is 332nm, the wavelength range is 200cm -1 Up to 2000cm -1 Then Peakfit software was used for fitting analysis to obtain the network structure.
[0061] On the other hand, the glass powder corresponding to each oxide composition can be subjected to a differential scanning calorimetry test to obtain the temperature performance of the sealing material. The temperature performance in the disclosed embodiment may include a glass transition temperature and / or a glass softening temperature. Among them, the parameters of the differential scanning calorimetry test include: a heating rate of 10°C / min, and a heating range of room temperature to 1200°C.
[0062] Next, the network structure composition and temperature performance of each sealing material obtained through multiple process tests can be used for data fitting to obtain the relationship between the network structure composition and temperature performance of the sealing material. Specifically, Origin software can be used to draw a graph to obtain a visual result.
[0063] In order to illustrate the sealing material analysis scheme of the present disclosure in more detail, examples 1 and 2 are described in detail below.
[0064] The oxide components of the oxide compositions of Examples 1 and 2 are configured as shown in Table 1 of the composition table (wt %):
[0065] Table 1
[0066]
[0067] The processing procedures of Example 1 and Example 2 are described below in conjunction with the accompanying drawings.
[0068] Example 1
[0069] First, the melting temperature was calculated. Specifically, in FactSage software, the FToxid database was selected, the total mass was calculated as 100 g, and in the Equilib module, after the components of Example 1 in Table 1 were input, Slag-liq was selected as the basic phase, and the initial melting temperature of the oxide composition was calculated to be 639.18°C and the complete melting temperature was 1227.28°C. Figure 2 This is a diagram of the software interface for calculating the melting start temperature in Example 1. Figure 3 This is a diagram of the software interface for calculating the complete melting temperature of Example 1.
[0070] It should be noted that the melting temperature applied to the above-mentioned actual process of the present disclosure may be a complete melting temperature.
[0071] At the same time, a mixing process can be performed. Specifically, according to the oxide composition of Example 1 in Table 1, the total mass is controlled to be, for example, 100 g, that is, 20 g of SiO2, 50 g of B2O3, 10 g of MgO, 15 g of SrO and 5 g of MgO are taken respectively, and they are put into a mixer and mixed for 30 minutes to obtain a uniform oxide composition powder.
[0072] Next, a total of 100 g of the above oxide composition was placed in an alumina crucible, and the crucible was placed in a muffle furnace, heated to 1100°C at a heating rate of 8°C / min, kept warm for 1 hour, and then heated to 1450°C at a heating rate of 5°C / min, and kept warm for 2 hours to obtain glass liquid.
[0073] At the same time, aluminum foil is used to line the bottom of the iron bucket to prevent contamination. After the heat preservation is completed, the glass liquid is poured into an iron bucket filled with deionized water at high temperature for water quenching to obtain glass slag. The glass slag is taken out and placed in an oven at 70°C for drying for 24 hours.
[0074] Subsequently, the dried glass slag is placed in an alumina ball mill with a ball-to-material ratio of 4:1, and ball milled at a speed of 400 r / min for 4 hours, and then passed through a 200-mesh sieve to obtain glass powder.
[0075] Then, the glass powder is tested. Specifically, the glass powder can be tested by X-ray photoelectron spectroscopy, Raman spectroscopy and differential scanning calorimetry.
[0076] Figure 4 A schematic diagram showing the fitting results of the X-ray photoelectron spectrum of Example 1 of the present disclosure is shown. Specifically, the results can be analyzed using AVANTAGE software, and the analysis steps may include: selecting a peak range → selecting the position of the oxygen peak → fitting → exporting the results, and then obtaining the proportions of different oxygen structure types.
[0077] The oxygen structure of the embodiment of the present disclosure includes bridging oxygen (BO) and non-bridging oxygen (NBO), and the binding energies of bridging oxygen and non-bridging oxygen are about 532.12eV and 531eV, respectively. Figure 4 , combined with the original line and the above standards of bridging oxygen binding energy 532.12eV and non-bridging oxygen binding energy 531eV, the corresponding curve areas are obtained, and then the ratio of bridging oxygen to non-bridging oxygen (wt%) can be obtained. Figure 4 The results shown show that the bridging oxygen in Example 1 is 24.31 wt %, the non-bridging oxygen is 75.69 wt %, and the ratio of non-bridging oxygen to bridging oxygen is 3.11.
[0078] Figure 5A schematic diagram showing the fitting results of the Raman spectrum of Example 1 of the present disclosure is shown. Specifically, the Raman results can be analyzed using Peakfit software, and the analysis steps may include: data import → area standardization → baseline removal → peak search → fitting → iteration → export results to obtain the proportion of the glass network structure.
[0079] refer to Figure 5 In the fitting process, for the peak types, they correspond to SiO4 with zero-bridge oxygen 4− (Q 0 )、Si2O7 6− Dimer structure (Q 1 )、chain structural unit Si2O6 4− (Q 2 ) and sheet-like structural unit Si2O5 2− (Q 3 ). In addition, at 1150 cm −1 The peaks near the BO-Si structure correspond to the curve area corresponding to them, and Q 2 Structure, Q 3 Structure and the ratio of BO-Si structure (wt%). Figure 5 The results shown show that the Q of Example 1 2 The structure is 15.98wt%, Q 3 The structure is 53.55wt%, the BO-Si structure is 30.47wt%, and the Q 2 Structure and Q 3 The ratio of the structure is 0.29.
[0080] Figure 6 A schematic diagram of a differential scanning calorimetry (DSC) DSC curve of Example 1 of the present disclosure is shown. Through analysis, it can be determined that the glass transition temperature Tg is 630.3°C and the glass softening temperature Ts is 756.4°C.
[0081] Therefore, Example 1 can obtain a set of corresponding relationships between oxygen structure, network structure composition and temperature performance.
[0082] Example 2
[0083] First, the melting temperature was calculated. Specifically, in FactSage software, the FToxid database was selected, the total mass was calculated as 100 g, and in the Equilib module, after the components of Example 2 in Table 1 were input, Slag-liq was selected as the basic phase, and the initial melting temperature of the oxide composition was calculated to be 632.87°C and the complete melting temperature was 1227.21°C. Figure 7 This is the software interface diagram for calculating the melting start temperature of Example 2. Figure 8This is the software interface diagram for calculating the complete melting temperature of Example 2.
[0084] It should be noted that the melting temperature applied to the above-mentioned practical process of the present disclosure is the complete melting temperature.
[0085] At the same time, a mixing process can be performed. Specifically, according to the oxide composition of Example 2 in Table 1, the total mass is controlled to be, for example, 100 g, that is, 25 g of SiO2, 45 g of B2O3, 10 g of MgO, 15 g of SrO and 5 g of MgO are taken respectively, and they are put into a mixer and mixed for 30 minutes to obtain a uniform oxide composition powder.
[0086] Next, a total of 100 g of the above oxide composition was placed in an alumina crucible, and the crucible was placed in a muffle furnace, heated to 1100°C at a heating rate of 8°C / min, kept warm for 1 hour, and then heated to 1450°C at a heating rate of 5°C / min, and kept warm for 2 hours to obtain glass liquid.
[0087] At the same time, aluminum foil is used to line the bottom of the iron bucket to prevent contamination. After the heat preservation is completed, the glass liquid is poured into an iron bucket filled with deionized water at high temperature for water quenching to obtain glass slag. The glass slag is taken out and placed in an oven at 70°C for drying for 24 hours.
[0088] Subsequently, the dried glass slag is placed in an alumina ball mill with a ball-to-material ratio of 4:1, and ball milled at a speed of 400 r / min for 4 hours, and then passed through a 200-mesh sieve to obtain glass powder.
[0089] Then, the glass powder is tested. Specifically, the glass powder can be tested by X-ray photoelectron spectroscopy, Raman spectroscopy and differential scanning calorimetry.
[0090] Fig. 9 A schematic diagram showing the fitting results of the X-ray photoelectron spectrum of Example 2 of the present disclosure is shown. Specifically, the results can be analyzed using AVANTAGE software, and the analysis steps may include: selecting a peak range → selecting the position of the oxygen peak → fitting → exporting the results, and then obtaining the proportions of different oxygen structure types.
[0091] The oxygen structure of the embodiment of the present disclosure includes bridging oxygen (BO) and non-bridging oxygen (NBO), and the binding energies of bridging oxygen and non-bridging oxygen are about 532.12eV and 531eV, respectively. Fig. 9 , combined with the original line and the above-mentioned standard of bridging oxygen binding energy 532.12eV and non-bridging oxygen binding energy 531eV, the corresponding curve area can be obtained, and then the ratio of bridging oxygen and non-bridging oxygen (wt%) can be obtained. Fig. 9The results shown show that the bridging oxygen in Example 2 is 27.80 wt %, the non-bridging oxygen is 72.20 wt %, and the ratio of non-bridging oxygen to bridging oxygen is 2.59.
[0092] Fig.10 A schematic diagram showing the fitting results of the Raman spectrum of Example 2 of the present disclosure is shown. Specifically, the Raman results can be analyzed using Peakfit software, and the analysis steps may include: data import → area standardization → baseline removal → peak search → fitting → iteration → export results to obtain the proportion of the glass network structure.
[0093] refer to Fig.10 In the fitting process, for the peak types, they correspond to SiO4 with zero-bridge oxygen 4− (Q 0 )、Si2O7 6− Dimer structure (Q 1 )、chain structural unit Si2O6 4− (Q 2 ) and sheet-like structural unit Si2O5 2− (Q 3 ). In addition, at 1150 cm −1 The nearby peaks correspond to the BO-Si structure. Corresponding to their curve areas, Q 2 Structure, Q 3 Structure and the ratio of BO-Si structure (wt%). Fig.10 The results shown show that the Q of Example 2 2 The structure is 11.53wt%, Q 3 The structure is 63.11wt%, the BO-Si structure is 25.36wt%, and the Q 2 Structure and Q 3 The ratio of the structure is 0.18.
[0094] Fig.11 A schematic diagram of a differential scanning calorimetry (DSC) DSC curve of Example 2 of the present disclosure is shown. Through analysis, it can be determined that the glass transition temperature Tg is 621.3°C and the glass softening temperature Ts is 714.8°C.
[0095] Therefore, Example 2 can obtain another set of corresponding relationships between oxygen structure, network structure composition and temperature performance.
[0096] By combining the process test results for multiple oxide compositions including the results of the above-mentioned Example 1 and Example 2, data fitting can be performed to determine the relationship between the oxygen structure and the temperature performance, as well as the relationship between the network structure composition and the temperature performance. Specifically, Fig.12A schematic diagram showing the relationship between the fitted oxygen structure and temperature performance of an embodiment of the present disclosure is shown, wherein the abscissa represents the ratio of non-bridging oxygen to bridging oxygen, and the ordinate represents temperature. Fig.12 In the abscissa, as described in Example 1, the bridging oxygen is 24.31 wt %, the non-bridging oxygen is 75.69 wt %, and the ratio of the non-bridging oxygen to the bridging oxygen is 3.11. Fig.13 A schematic diagram showing the relationship between the network structure composition and temperature performance of the embodiment of the present disclosure, wherein the abscissa represents Q 2 Structure and Q 3 The ratio of the structure, the vertical axis represents the temperature. Fig.13 The horizontal axis in the example described in Example 1 is Q 2 The structure is 15.98wt%, Q 3 The structure is 53.55wt%, Q 2 Structure and Q 3 The ratio of the structure is 0.29.
[0097] It should be noted that after the above relationship is determined, it can be regulated based on the oxygen structure according to the application requirements of the temperature performance of the sealing material.
[0098] It should be noted that although the steps of the method in the present disclosure are described in a specific order in the drawings, this does not require or imply that the steps must be performed in this specific order, or that all the steps shown must be performed to achieve the desired results. Additionally or alternatively, some steps may be omitted, multiple steps may be combined into one step, and / or one step may be decomposed into multiple steps, etc.
[0099] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.
[0100] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing what is disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary technical means in the art that are not disclosed in the present disclosure. The specification and embodiments are to be considered merely as exemplary, and the true scope and spirit of the present disclosure are indicated by the claims.
[0101] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.
Claims
1. A sealing material analysis method, characterized in that: include: Calculating the melting temperature of each of the plurality of oxide compositions using thermochemical calculation software, wherein the contents of the oxides contained in the oxide compositions are not completely the same, and the oxide compositions contain 20 wt % to 40 wt % of SiO2, 30 wt % to 60 wt % of B2O3, 10 wt % to 30 wt % of SrO, 5 wt % to 20 wt % of MgO, and 1 wt % to 5 wt % of Na2O; Melting the oxide composition at a target temperature to obtain a glass melt; wherein the target temperature is higher than the melting temperature of the oxide composition; The glass liquid is subjected to water quenching and drying to obtain glass slag; Ball milling the glass slag to obtain glass powder; Performing an X-ray photoelectron spectroscopy test on the glass powder corresponding to each of the oxide compositions to obtain the oxygen structure of the sealing material, wherein the oxygen structure includes bridging oxygen and non-bridging oxygen; Performing a differential scanning calorimetry test on the glass powder corresponding to each of the oxide compositions to obtain the temperature performance of the sealing material; wherein the temperature performance includes a glass transition temperature and / or a glass softening temperature; Using the ratio of non-bridging oxygen to bridging oxygen and the temperature performance of each of the sealing materials to perform data fitting, so as to obtain the relationship between the ratio of non-bridging oxygen to bridging oxygen and the temperature performance of the sealing material; The sealing material analysis method further comprises: The glass powder corresponding to each oxide composition is subjected to Raman spectroscopy test to obtain the network structure composition of the sealing material, wherein the network structure composition includes Q 2 Structure and Q 3 structure; The Q of each sealing material is used 2 Structure and Q 3 The ratio of the structure and the temperature performance are fitted to obtain the Q of the sealing material. 2 Structure and Q 3 Relationship between the ratio and temperature performance of the structure.
2. The sealing material analysis method according to claim 1, characterized in that: The sealing material analysis method further comprises: Obtain multiple oxides in proportion; The plurality of oxides are put into a mixer for mechanical mixing to obtain the oxide composition.
3. The sealing material analysis method according to claim 1, characterized in that: The temperature difference between the target temperature and the melting temperature of the oxide composition is greater than 100°C to 200°C.
4. The sealing material analysis method according to claim 1 or 3, characterized in that: Melting the oxide composition at a target temperature to obtain a glass melt comprises: The oxide composition is melted at a target temperature for 2 hours to 6 hours using an alumina crucible or a magnesia crucible to obtain the glass liquid.
5. The sealing material analysis method according to claim 1, characterized in that: The glass liquid is subjected to water quenching and drying to obtain glass slag, comprising: The glass liquid is quenched with deionized water and dried to obtain the glass slag.
6. The sealing material analysis method according to claim 1, characterized in that: The ball milling process uses alumina balls and alumina ball milling jars. The diameters of the alumina balls include 2 mm, 5 mm and 8 mm. The ball-to-material ratio is 3:1 to 5:
1. The rotation speed of the ball milling process is 200 r / min to 400 r / min. The ball milling time is 4 h to 10 h.
Citation Information
Patent Citations
Predicating method for transformation temperature and hardness of glass
CN104062422A
Method for improving 2microm waveband fluorescence emission of rare earth ion doped germanate glass
CN110510875A
Li-Al-Si photosensitive glass and preparation method thereof
CN111718120A
Tellurate glass as well as preparation method and application thereof
CN117964233A
A zirconia doping of soda-lime glass
TW202021920A