Dry film for electroplating copper pillars and IC substrate copper pillars
By adopting a multi-layer dry film and gradually increasing the dosage of photosensitizer, the energy loss and side corrosion problems caused by the existing dry film thickness are solved, the technical requirements for the perpendicularity of the side wall of the copper column are ensured, and electronic components are improved reliability and interconnect performance.
Patent Information
- Application Number
- CN202410864705.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-01
AI Technical Summary
The thick dry film thickness causes a large energy loss when cured light passes through the film layer. The energy of the light ray is attenuated during the exposure process, causing the bottom side corrosion, which cannot meet the technical requirements of the perpendicularity of the copper column side wall, affecting the reliability of electronic components. .
Using dry films with at least three layers of structure, each layer has a thickness of no more than 20μm and a total thickness of between 50-200μm. By gradually increasing the amount of photosensitizer in each layer of dry film, the curing degree of each layer of dry film is ensured in the exposure process. Consistently, HEMA-IPDI-R-IPDI-HEMA photopolymerized monomer is used to improve the flexibility and deep curing ability of the dry film.
The uniform thickness and rapid drying of the dry film are achieved, side corrosion is avoided, and the verticality of the side wall of the copper column is 0.9
Smart Images

Figure CN118393813B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials for patterned surface photolithography of photoresists, and in particular to a dry film for electroplating copper pillars and an IC carrier copper pillar. Background Art
[0002] With the advancement and development of science and technology, the number of external leads and the density of copper interconnect wires of integrated circuit (IC) chip packaging are getting higher and higher. The traditional solder bump packaging process is to remelt the solder bump and reflow solder it to the substrate, which will cause deformation, making the solder ball spacing inconsistent and difficult to detect and control. During the packaging process, the bottom filling between the chip and the substrate mainly flows to the gap with a larger solder ball spacing, and the gap with a smaller spacing is not filled. The resulting voids have a negative effect on the reliability of electronic devices.
[0003] Copper pillar bump technology is a new generation of chip interconnect technology. Copper pillar bumps are composed of copper pillars and solder caps. The solder cap can be made of commonly used solder. Due to the use of a small amount of solder, the deformation of copper pillar bumps during interconnection is significantly reduced. During the melting and reflow process, the copper pillar bumps almost maintain their shape. The consistent spacing between copper pillar bumps reduces the voids produced after the bottom is filled, which means higher process quality and electronic device reliability. In addition, copper pillar bumps have a consistent height and the spacing can be smaller, which can realize fine pitch array interconnection, improve the electrical performance of the interconnection, and improve the heat dissipation performance.
[0004] The preparation method of copper pillar bump is usually as follows Figure 1 As shown, a layer of dry film is first covered on the copper foil carrier, and the pattern is transferred through exposure and development processes to obtain a cylindrical pit with a copper foil carrier at the bottom and dry film around it. Then, electroplating deposition is performed in the cylindrical pit to form a copper column. Finally, the dry film is removed from the copper foil carrier to obtain a copper column bump.
[0005] The manufacture of copper pillars usually requires the use of a dry film of sufficient thickness, which is usually greater than 50 μm, far exceeding the general dry film thickness level. The existing dry film has the following problems: (1) The dry film is relatively thick and is prone to flow during the coating process, making it difficult to control the thickness uniformity. In addition, the bottom solvent is difficult to fully evaporate and the drying speed is slow. (2) During the exposure process, the energy of the light passing through the dry film is attenuated, which can easily cause the top and bottom of the dry film to have inconsistent curing degrees, causing excessive development of the bottom during the subsequent development process, forming bottom side etching, and ultimately causing the verticality T of the copper pillar side wall formed by electroplating (i.e., the ratio of the top diameter to the bottom diameter of the copper pillar) to fail to meet the technical requirement of 0.9<T≤1, and thus the reliability of high-density interconnected electronic components cannot be guaranteed. (3) In order to obtain a copper pillar of sufficient height, long-term electroplating deposition is required. The dry film is prone to fall off under long-term electroplating conditions and is prone to precipitating organic matter. Summary of the invention
[0006] The present invention provides a dry film for electroplating copper pillars and an IC carrier copper pillar, so as to solve the technical problems in the prior art that the single-layer dry film is too thick, resulting in large energy loss when the curing light passes through the film layer, and the energy of the light passing through the dry film is attenuated during the exposure process, resulting in bottom side corrosion.
[0007] According to one aspect of the present invention, a dry film for electroplating copper pillars is provided, wherein the dry film has at least three layers, the total thickness of which is between 50 and 200 μm, and the thickness of each layer of the dry film does not exceed 20 μm;
[0008] The raw materials of each layer of the dry film include: 45-65 parts by weight of alkali-soluble resin, 30-50 parts by weight of photopolymerization monomer, 2-4 parts by weight of photoinitiator and 0.2-1.8 parts by weight of photosensitizer; the photopolymerization monomer includes HEMA-IPDI-R-IPDI-HEMA, the weight average molecular weight of R is 500-5000 g / mol, and R is selected from one of polyethylene glycol, polypropylene glycol, polybutylene glycol, polytetramethylene ether glycol, polycaprolactone glycol and polybutylene adipate-1,4-diol; the mass percentage of HEMA-IPDI-R-IPDI-HEMA in the photopolymerization monomer is 20-40%;
[0009] The structural formula of HEMA-IPDI-R-IPDI-HEMA is as follows:
[0010]
[0011] The content of the photosensitizer in each layer of dry film increases from top to bottom, and in two adjacent layers of dry film, the mass ratio of the photosensitizer in the lower dry film to that in the upper dry film is 1.05-1.4.
[0012] Furthermore, the thickness of each layer of the dry film is between 5-20 μm, and the total thickness of the dry film is between 50-200 μm.
[0013] Furthermore, the total thickness of the dry film is between 80-150 μm;
[0014] Each layer of the alkali-soluble resin comprises (meth)acrylic acid, (meth)acrylates and aromatic compounds in a mass ratio of (15-40): (20-30): (20-55);
[0015] The (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate and / or butyl (meth)acrylate;
[0016] The aromatic compounds include phenoxyethyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, styrene and / or o-phenylphenoxyethyl acrylate.
[0017] Furthermore, the mass percentage of the HEMA-IPDI-R-IPDI-HEMA in the photopolymerizable monomer is 30%.
[0018] Furthermore, the photopolymerizable monomer also includes a vinyl-containing (meth)acrylate compound, and the vinyl-containing (meth)acrylate compound includes one or more of ethoxy nonylphenol (meth)acrylate, propoxy nonylphenol (meth)acrylate, ethoxy bisphenol A di(meth)acrylate, ethoxy di(meth)acrylate, propoxy di(meth)acrylate, ethoxy trimethylolpropane tri(meth)acrylate or ethoxy pentaerythritol tetra(meth)acrylate.
[0019] Further, the photoinitiator is a triaryl imidazole dimer derivative, and the photoinitiator includes any one or more of 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer, and 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole.
[0020] Furthermore, the photosensitizer is an anthracene and / or benzophenone compound.
[0021] Furthermore, the photosensitizer is one or more of 9,10-dibutoxyanthracene, 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-diphenylanthracene, and tetraethyl Michler's ketone.
[0022] Furthermore, the raw materials of the dry film also include at least one of a light stabilizer, a heat stabilizer, an antioxidant, a photocolor developer, a photoacid generator, a plasticizer, a pigment, a filler, a defoamer, and a leveling agent.
[0023] According to another aspect of the present invention, there is provided an IC carrier copper column prepared from the dry film for electroplating copper columns.
[0024] The present invention has the following beneficial effects:
[0025] (1) The present invention measures the absorptivity of each layer of dry film to the curing light by an ultraviolet-visible spectrophotometer, thereby determining the addition ratio of the photosensitizer in each layer of dry film, so that the amount of the photosensitizer increases gradually from top to bottom, and at the same time, in two adjacent layers of dry film, the mass ratio of the photosensitizer in the lower dry film to the upper dry film is 1.05-1.4, which makes up for the energy attenuation of the curing light when passing through the dry film, so that the curing degree of each layer of dry film is consistent in the exposure process, thereby avoiding the side etching phenomenon in the development process, and ensuring that the verticality T of the side wall of the prepared copper column satisfies 0.9<T≤1.
[0026] (2) The present invention adopts multi-layer coating, and the dry film has at least three layers, and the total thickness is between 50-200 μm. The thickness of each layer of dry film does not exceed 20 μm. Since the thickness of each coating layer is relatively thin, it is not easy to flow during the coating process, the film thickness is uniform, and the drying speed is fast, and the bottom layer is fully dried. At the same time, the problem of too thick film layer thickness and large energy loss when the curing light passes through these thick film layers is avoided.
[0027] (3) The present invention selects HEMA-IPDI-R-IPDI-HEMA photopolymerizable monomer, whose R group contains a flexible chain segment, which can improve the flexibility of the dry film. In addition, this photopolymerizable monomer has a high refractive index and is not easy to crystallize, which helps light to penetrate and improves the deep curing ability of the dry film.
[0028] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0030] Figure 1 Schematic diagram of the preparation method of copper pillars of IC carrier board;
[0031] Figure 2 Schematic diagram of the method for calculating the verticality of the sidewall of the copper pillar of the IC carrier;
[0032] Figure 3 This is a microscopic photograph of a cross section of the copper pillar of the IC carrier prepared in Example 1;
[0033] Figure 4 This is a cross-sectional microscope photograph of the copper pillar of the IC carrier prepared in Comparative Example 2. DETAILED DESCRIPTION
[0034] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. However, the present invention can be implemented in many different ways as defined and covered below.
[0035] According to an embodiment of the first aspect of the present invention, there is provided a dry film for electroplating copper pillars, wherein the dry film has at least three layers, the total thickness of which is between 50 and 200 μm, and the thickness of each layer of the dry film does not exceed 20 μm;
[0036] The raw materials of each layer of the dry film include: 45-65 parts by weight of alkali-soluble resin, 30-50 parts by weight of photopolymerization monomer, 2-4 parts by weight of photoinitiator and 0.2-1.8 parts by weight of photosensitizer; the photopolymerization monomer includes HEMA-IPDI-R-IPDI-HEMA, the weight average molecular weight of R is 500-5000 g / mol, and R is selected from one of polyethylene glycol, polypropylene glycol, polybutylene glycol, polytetramethylene ether glycol, polycaprolactone glycol and polybutylene adipate-1,4-diol; the mass percentage of HEMA-IPDI-R-IPDI-HEMA in the photopolymerization monomer is 20-40%;
[0037] The structural formula of HEMA-IPDI-R-IPDI-HEMA is as follows:
[0038]
[0039] The content of the photosensitizer in each layer of dry film increases from top to bottom, and in two adjacent layers of dry film, the mass ratio of the photosensitizer in the lower dry film to that in the upper dry film is 1.05-1.4.
[0040] The present invention uses multi-layer coating for thick dry films with a thickness between 50-200 μm, and limits the thickness of each layer of dry film to no more than 20 μm. The number of coating layers can be set according to the thickness of the dry film. The thicker the thickness, the more layers are set. For example, a dry film with a thickness of 50-60 μm is coated with at least three layers, a dry film with a thickness of 60-80 μm (excluding 60 μm) is coated with at least four layers, a dry film with a thickness of 80-100 μm (excluding 80 μm) is coated with at least five layers, and so on.
[0041] The present invention adopts multi-layer coating, each coating layer is thin, flow is not easy to occur during the coating process, the film thickness is uniform, the drying speed is fast, and the bottom layer is fully dried.
[0042] The present invention selects HEMA-IPDI-R-IPDI-HEMA photopolymerizable monomer, whose R group contains a flexible chain segment, so that the flexibility of the dry film can be improved. In addition, the photopolymerizable monomer has a high refractive index and is not easy to crystallize, which is conducive to the transmission of light and improves the deep curing ability of the dry film.
[0043] As a preferred embodiment, the thickness of each dry film layer is between 5-20 μm, more preferably 10-15 μm, and the total thickness of the dry film is between 50-200 μm, more preferably 80-150 μm, and further preferably 100 μm. The thickness of each layer of dry film can be the same or different, but the difference in thickness between two adjacent layers does not exceed 10 μm.
[0044] As a preferred embodiment, in two adjacent dry films, the mass ratio of the photosensitizer in the lower dry film to that in the upper dry film is 1.05-1.3, more preferably 1.05-1.2, and further preferably 1.1-1.15.
[0045] The present invention adopts a multi-layer coating technology and measures the absorption rate of each layer of dry film to the curing light by an ultraviolet visible spectrophotometer, thereby determining the addition ratio of the photosensitizer in each layer of dry film, so that the amount of the photosensitizer is gradually increased from top to bottom, which makes up for the energy attenuation of the curing light when passing through the dry film, so that the curing degree of each layer of dry film is consistent in the exposure process (that is, the absorption rate of the dry film to the curing light is consistent, and consistency does not mean that each layer is completely the same, as long as the difference between each layer does not exceed ±10%, the requirement can be met), thereby avoiding the side etching phenomenon in the development process, and ensuring that the verticality T of the side wall of the prepared copper column (that is, the ratio of the top diameter L2 to the bottom diameter L1 of the copper column) satisfies 0.9<T≤1.
[0046] As a preferred embodiment, the mass fraction of the alkali-soluble resin is preferably any one of 47 parts, 49 parts, 51 parts, 53 parts, 55 parts, 57 parts, 59 parts, 61 parts, 63 parts, etc.
[0047] As a preferred embodiment, the mass fraction of the photopolymerizable monomer is preferably any one of 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 46 parts, 48 parts, etc.
[0048] As a preferred embodiment, the mass fraction of the photoinitiator is preferably 3 parts.
[0049] In this embodiment, each layer of the alkali-soluble resin comprises (meth)acrylic acid, (meth)acrylates and aromatic compounds in a mass ratio of (15-40): (20-30): (20-55);
[0050] The (meth)acrylates include one or more of methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate;
[0051] The aromatic compound includes one or more of phenoxyethyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, styrene, and o-phenylphenoxyethyl acrylate.
[0052] The present invention adopts an alkali-soluble polymer resin having (meth)acrylate structural units and aromatic compound structural units, has strong chemical resistance and good adhesion, and can meet the electroplating resistance requirements of dry films under long-term electroplating conditions.
[0053] As a preferred embodiment, the alkali-soluble resin has a weight average molecular weight between 10,000 and 50,000, and an acid value between 130 and 180 mgKOH / g.
[0054] In this embodiment, the photopolymerizable monomer includes HEMA-IPDI-R-IPDI-HEMA, the weight average molecular weight of R is 500-5000 g / mol, and R is selected from one of polyethylene glycol, polypropylene glycol, polybutylene glycol, polytetramethylene ether glycol, polycaprolactone glycol, and polybutylene adipate-1,4-diol; the mass percentage of HEMA-IPDI-R-IPDI-HEMA in the photopolymerizable monomer is 20-40%;
[0055] The mass percentage of the HEMA-IPDI-R-IPDI-HEMA in the photopolymerizable monomer is 30%.
[0056] As a preferred embodiment, the weight average molecular weight of R is 800-4000 g / mol, more preferably 800-3000 g / mol, more preferably 1000-2000 g / mol, and further preferably 1000-1500 g / mol.
[0057] In order to meet the demand that the dry film for electroplating copper pillars has a certain resolving power when the thickness is high, in the present invention, an alkali-soluble resin with a high benzene ring content is selected. However, this selection results in the overall hardness of the dry film, which may cause insufficient adhesion between each layer during multi-layer coating. By selecting HEMA-IPDI-R-IPDI-HEMA photopolymerizable monomer, the R group of which contains a flexible segment, the flexibility of the dry film can be improved. In addition, this photopolymerizable monomer has a higher refractive index and is not easy to crystallize, which helps the transmission of light and improves the deep curing ability of the dry film.
[0058] In this embodiment, the photopolymerizable monomer further comprises a vinyl-containing (meth)acrylate compound, and the vinyl-containing (meth)acrylate compound comprises one or more of ethoxylated nonylphenol (meth)acrylate, propoxylated nonylphenol (meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, ethoxylated di(meth)acrylate, propoxylated di(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, and ethoxylated pentaerythritol tetra(meth)acrylate. Further preferably, the photopolymerizable monomer is selected from one or more of ethoxylated di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, ethoxylated nonylphenol (meth)acrylate, and ethoxylated trimethylolpropane tri(meth)acrylate.
[0059] In this embodiment, the photoinitiator is a triaryl imidazole dimer derivative, and the photoinitiator includes any one or more of 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer, and 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole.
[0060] In this embodiment, the photosensitizer is an anthracene and / or benzophenone compound, preferably one or more of 9,10-dibutoxyanthracene, 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-diphenylanthracene, and tetraethyl Michler's ketone.
[0061] In this embodiment, the raw materials of the dry film further include at least one of a light stabilizer, a heat stabilizer, an antioxidant, a photochromic agent, a photoacid generator, a plasticizer, a pigment, a filler, a defoamer, and a leveling agent.
[0062] In this embodiment, each dry film layer is formed by coating each layer of resist coating liquid and then drying it.
[0063] As a preferred embodiment, the viscosity of each layer of dry film resist coating liquid at 25° C. is 500-4000 mPa·s, more preferably 800-3000 mPa·s, and even more preferably 1000-2000 mPa·s.
[0064] As a preferred embodiment, the solvent in each layer of the dry film resist coating solution is selected from one or a combination of ketone solvents or alcohol solvents.
[0065] According to another embodiment of the present invention, a method for preparing copper pillars of an IC carrier is provided, comprising the following steps: forming the electroplated copper pillars on a copper foil carrier using a dry film, then irradiating a portion of the dry film with curing light to form a cured portion, then removing the uncured portion of the dry film from the copper foil carrier to form a resist pattern, electroplating and depositing copper pillars in pits of the resist pattern, and then removing the resist pattern to form copper pillars of an IC carrier.
[0066] According to yet another embodiment of the present invention, there is provided an IC carrier copper column prepared by the above preparation method.
[0067] See also Figures 2 to 4 ,
[0068] Figure 2 Schematic diagram of the method for calculating the verticality of the sidewall of the copper pillar of the IC carrier;
[0069] Figure 3 This is a microscopic photograph of a cross section of the copper pillar of the IC carrier prepared in Example 1;
[0070] Figure 4 This is a cross-sectional microscope photograph of the copper pillar of the IC carrier prepared in Comparative Example 2.
[0071] Example 1
[0072] The total thickness of the dry film provided in this embodiment is 100 μm. Five layers of coating are used, and the thickness of each dry film layer is 20 μm. Calculated by weight, the raw materials of the surface dry film include: 52 parts of alkali-soluble resin, 42 parts of photopolymerizable monomers, 3.0 parts of photoinitiator, 0.5 parts of photosensitizer, and 2.5 parts of additives.
[0073] The alkali-soluble resin is an acrylate copolymer obtained by solution polymerization of methacrylic acid, methyl methacrylate and benzyl methacrylate in a mass ratio of 24:10:66 in acetone solvent, with a solid content of 40%, a weight average molecular weight of 40,000 and an acid value of 156 mgKOH / g.
[0074] The photopolymerizable monomer is a mixture of 10(ethoxy)bisphenol A dimethacrylate, 4(ethoxy)bisphenol A dimethacrylate, 3(ethoxy)trimethylolpropane triacrylate and HEMA-IPDI-R-IPDI-HEMA, and the mass ratio of the four is 1.8:1:0.4:0.8.
[0075] Among them, 10 (ethoxy) bisphenol A dimethacrylate, 4 (ethoxy) bisphenol A dimethacrylate, and 3 (ethoxy) trimethylolpropane triacrylate were all purchased from Sartomer Guangzhou Chemical Co., Ltd.
[0076] The preparation method of HEMA-IPDI-R-IPDI-HEMA comprises the following steps:
[0077] 150 parts of R were added to the reaction kettle, followed by 66.5 parts of IPDI, and then 40 parts of toluene were added to react at 60°C for 2 hours, and then a mixture of 0.135 parts of dibutyltin laurate and 45 parts of HEMA was added dropwise for 60 minutes, and then reacted at 75°C for 4 hours, and the -NCO content was measured to be less than 0.1wt%, thus obtaining HEMA-IPDI-R-IPDI-HEMA, wherein R is polypropylene glycol with a weight average molecular weight of 1000 g / mol.
[0078] The photoinitiator is 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer.
[0079] The photosensitizer is 9,10-dibutoxyanthracene.
[0080] The additives are 0.45 parts by mass of leuco crystal violet, 0.02 parts by mass of 4-tert-butylphenol, 0.03 parts by mass of malachite green and 2 parts by mass of p-toluenesulfonamide, all of which are purchased from Anhui Zesheng Technology Co., Ltd.
[0081] The solvent is 15 parts by weight, and acetone, toluene and methanol are used in a weight ratio of 4:6:5.
[0082] Preparation of surface resist coating liquid: After dissolving the above-mentioned photoinitiator, photosensitizer and auxiliary agent in a solvent, add alkali-soluble resin and photopolymerizable monomer, and stir evenly.
[0083] Preparation of the second to fifth layers of resist coating liquid: except that the amounts of photosensitizer are 0.6, 0.7, 0.8 and 0.9 parts by weight respectively, the other ingredients are the same as those of the surface layer resist coating liquid.
[0084] Preparation of photosensitive dry film:
[0085] The above-mentioned surface anti-etching agent coating liquid was coated on a 15 μm thick polyethylene terephthalate support film using a coating device (model: AB4220, TQC Company of the Netherlands), and baked at 80°C for 15 min to form a 20 μm thick surface dry film. Then, the second to fifth layers of anti-etching coating liquid were coated on the surface dry film in turn, and baked at 80°C for 15 min to form second to fifth layers of dry films with a thickness of 20 μm, respectively, and then covered with a polyethylene film for protection to obtain a photosensitive dry film.
[0086] Preparation of copper column:
[0087] Film lamination: A 35 μm thick copper-clad laminate laminated with a 1.2 mm thick rolled copper foil was preheated to 80°C, and the polyethylene protective film of the photosensitive dry film was peeled off while a hot roller laminator (model: CSL-M25E, Zhisheng Technology Co., Ltd.) was used to laminate the photosensitive dry film onto the copper-clad laminate at a roller temperature of 110°C, an air pressure of 0.35 MPa, and a lamination speed of 1.5 m / min to obtain a dry film-laminated substrate.
[0088] Exposure: A direct drawing exposure machine (model: MAS-04L10-8, Core Microelectronics Equipment Co., Ltd., main wavelength 405 nm) was used to expose the above-mentioned dry film-coated substrate at an energy level that made the number of residual stages after development of the Stouffer 41-stage exposure ruler reach 20, thereby obtaining a substrate with a cured film.
[0089] Development: After exposure, the polyethylene terephthalate support film is peeled off, and an alkali developer (a dry film developer manufactured by Guangzhou Julong Printing Equipment Co., Ltd.) is used to spray a 1wt% Na2CO3 aqueous solution at 30°C for twice the minimum development time to dissolve and remove the unexposed part of the photosensitive resin layer. After development, the substrate is washed with pure water for 1.5 times the development time, dehydrated with an air knife, and then dried with warm air to obtain a substrate with a resist pattern.
[0090] Depositing copper pillars: electroplating and depositing copper pillars in the pits of the resist pattern, and then removing the resist pattern to form copper pillars for the IC carrier.
[0091] Example 2
[0092] Except that the photosensitizer in Example 1 is replaced by 9,10-biphenylanthracene, other preparation conditions are the same as those in Example 1.
[0093] Example 3
[0094] Except that the photosensitizer in Example 1 was replaced by tetraethyl Michler's ketone, other preparation conditions were the same as those in Example 1.
[0095] Example 4
[0096] Except that the total thickness of the dry film in Example 1 is adjusted to 150 μm, the number of layers is adjusted to eight layers, the thickness of the dry film layers from top to bottom are 20 μm, 20 μm, 20 μm, 20 μm, 20 μm, 20 μm, 15 μm, and 15 μm, respectively, and the amount of photosensitizer in each dry film layer from top to bottom is adjusted to 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, and 1.2 parts by mass, respectively, the other preparation conditions are the same as those in Example 1.
[0097] Example 5
[0098] The preparation conditions are the same as those in Example 1, except that the total thickness of the dry film in Example 1 is adjusted to 200 μm, the number of layers is adjusted to ten, the thickness of each dry film layer is 20 μm, and the amount of photosensitizer in each layer of the dry film from top to bottom is adjusted to 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, and 1.4 parts by mass, respectively.
[0099] Example 6
[0100] Except that the total thickness of the dry film in Example 1 is adjusted to 50 μm, the number of layers is adjusted to three, the thickness of each dry film layer from top to bottom is 20 μm, 20 μm, and 10 μm, and the amount of photosensitizer in each dry film layer from top to bottom is adjusted to 1.3, 1.5, and 1.8 parts by mass, respectively, other preparation conditions are the same as those in Example 1.
[0101] Example 7
[0102] The other preparation conditions are the same as those in Example 1 except that the total thickness of the dry film in Example 1 is adjusted to 80 μm, the number of layers is adjusted to four, the thickness of each dry film layer from top to bottom is 20 μm, and the amount of photosensitizer in each dry film layer from top to bottom is adjusted to 0.2, 0.24, 0.3, and 0.4 parts by mass, respectively.
[0103] Example 8
[0104] The preparation conditions are the same as those in Example 1 except that the mass ratio of the photopolymerizable monomers 10 (ethoxy) bisphenol A dimethacrylate, 4 (ethoxy) bisphenol A dimethacrylate, 3 (ethoxy) trimethylolpropane triacrylate and HEMA-IPDI-R-IPDI-HEMA in Example 1 is adjusted to 1.4:1:0.4:1.2.
[0105] Example 9
[0106] The preparation conditions are the same as those in Example 1 except that the mass ratio of the photopolymerizable monomers 10 (ethoxy) bisphenol A dimethacrylate, 4 (ethoxy) bisphenol A dimethacrylate, 3 (ethoxy) trimethylolpropane triacrylate and HEMA-IPDI-R-IPDI-HEMA in Example 1 is adjusted to 1.2:0.8:0.4:1.6.
[0107] Comparative Example 1
[0108] Except that the dry film in Example 1 was adjusted to a single layer and the amount of the photosensitizer was 0.5 parts by mass, other preparation conditions were the same as those in Example 1.
[0109] Comparative Example 2
[0110] The other preparation conditions were the same as those in Example 1 except that the dry film in Example 1 was adjusted to a double layer, the thickness of each dry film was 50 μm, and the amounts of photosensitizer in the surface and bottom dry films were adjusted to 0.5 and 0.6 parts by weight, respectively.
[0111] Comparative Example 3
[0112] Except that the dry film thicknesses of the surface layer and the bottom layer in Comparative Example 2 are adjusted to 70 μm and 30 μm, respectively, other preparation conditions are the same as those in Comparative Example 2.
[0113] Comparative Example 4
[0114] Except that the dry film thicknesses of the surface layer and the bottom layer in Comparative Example 2 are adjusted to 30 μm and 70 μm, respectively, other preparation conditions are the same as those in Comparative Example 2.
[0115] Comparative Example 5
[0116] Except that the amount of photosensitizer in the bottom dry film in Comparative Example 2 is adjusted to 1.0 parts by mass, other preparation conditions are the same as those in Comparative Example 2.
[0117] Comparative Example 6
[0118] Except that the amount of photosensitizer in the bottom dry film in Comparative Example 2 is adjusted to 0.52 parts by mass, other preparation conditions are the same as those in Comparative Example 2.
[0119] Comparative Example 7
[0120] Except that the photopolymerizable monomer in Example 1 is replaced by a mixture of 10(ethoxy)bisphenol A dimethacrylate, 4(ethoxy)bisphenol A dimethacrylate, 3(ethoxy)trimethylolpropane triacrylate, and (ethoxy)nonylphenol acrylate in a mass ratio of 2:1:0.8:0.4 (purchased from Sartomer Guangzhou Chemical Co., Ltd.), the other preparation conditions are the same as those in Example 1.
[0121] Copper pillar sidewall verticality evaluation:
[0122] The copper pillars prepared above were polished and sliced to expose the top and bottom cross sections of the copper pillars. The cross sections of the copper pillars were observed using a SU1000 scanning electron microscope and evaluated according to the following evaluation criteria.
[0123] ■: The ratio of the top diameter to the bottom diameter of the copper column cross section satisfies 0.9<T≤1;
[0124] □: The ratio of the top diameter to the bottom diameter of the copper column cross section satisfies 0.85<T≤0.9;
[0125] ○: The ratio T of the top diameter to the bottom diameter at the copper column cross section satisfies 0.8<T≤0.85.
[0126] The above test results are summarized in Table 1 below.
[0127] Table 1 is a test summary table of Examples 1-5 and Comparative Examples 1-7
[0128]
[0129] From the above results, it can be seen that in Examples 1-9, by adopting multi-layer coating, limiting the thickness of a single-layer dry film, and increasing the amount of photosensitizer in each layer of the dry film from top to bottom, the curing degree of each layer of the dry film prepared is consistent, the dry film has good anti-side corrosion performance, and the verticality T of the side wall of the electroplated copper column obtained thereby satisfies 0.9<T≤1.
[0130] Comparative Example 1 uses the existing single-layer coating method. Since the film thickness is too thick, there is attenuation when the light passes through the dry film to the bottom layer, and the curing degree of the surface layer and the bottom layer are inconsistent. The dry film thus obtained has bottom side etching, resulting in poor verticality of the side wall of the prepared copper column.
[0131] Although Comparative Examples 2-4 use a double-layer coating method, which can solve the bottom layer side corrosion problem to a certain extent, the number of layers is too small, resulting in each layer or some of the film layers being too thick. When the curing light passes through these thicker film layers, the energy loss is large. No matter how the thickness ratio between the two layers or the photosensitizer ratio is adjusted, it is impossible to obtain an electroplated copper column with a side wall verticality exceeding 90%.
[0132] In addition, compared with Comparative Example 2, Comparative Example 3 reduces the thickness ratio of the bottom dry film, and Comparative Example 6 reduces the amount of photosensitizer in the bottom dry film, resulting in the bottom dry film's absorption rate of the curing light being insufficient to compensate for the energy attenuation of the curing light passing through the dry film. The dry film thus obtained still suffers from bottom side etching, and the verticality of the side wall of the prepared copper column does not reach 90%.
[0133] Compared with Comparative Example 2, the thickness ratio of the bottom dry film in Comparative Example 4 is too high, and the amount of photosensitizer in the bottom dry film in Comparative Example 5 is too high, both of which lead to the bottom dry film being too sensitive, the bottom curing being too high during the exposure process, and the top side etching occurring after development, which also leads to the verticality of the side wall of the prepared copper column being less than 90%.
[0134] In Comparative Example 7, the photopolymerizable monomer does not use HEMA-IPDI-R-IPDI-HEMA, and the obtained dry film resist has a poor refractive index and poor light transmittance, resulting in the verticality of the side wall of the prepared copper column not reaching 90%.
[0135] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A dry film for electroplating copper pillars, characterized in that: The dry film has at least three layers, with a total thickness of 50-200 μm, and the thickness of each layer of the dry film does not exceed 20 μm; The raw materials of each layer of the dry film include: 45-65 parts by weight of alkali-soluble resin, 30-50 parts by weight of photopolymerizable monomer, 2-4 parts by weight of photoinitiator and 0.2-1.8 parts by weight of photosensitizer; The alkali-soluble resin is an acrylate copolymer, which is obtained by solution polymerization of methacrylic acid, methyl methacrylate and benzyl methacrylate in a mass ratio of 24:10:66 in acetone solvent; The photopolymerizable monomer comprises HEMA-IPDI-R-IPDI-HEMA, wherein the first reaction raw material of the photopolymerizable monomer HEMA-IPDI-R-IPDI-HEMA is HEMA, the second reaction raw material is IPDI, the third reaction raw material is one of polyethylene glycol, polypropylene glycol, polybutylene glycol, polytetramethylene ether glycol, polycaprolactone glycol, and polybutylene adipate-1,4-diol, and the weight average molecular weight of R is 500-5000 g / mol; the mass percentage of the HEMA-IPDI-R-IPDI-HEMA in the photopolymerizable monomer is 20-40%; The structural formula of HEMA-IPDI-R-IPDI-HEMA is as follows: ; The content of the photosensitizer in each layer of dry film increases from top to bottom, and in two adjacent layers of dry film, the mass ratio of the photosensitizer in the lower dry film to that in the upper dry film is 1.05-1.
4.
2. The dry film for electroplating copper pillars according to claim 1, characterized in that: The thickness of each layer of the dry film is between 5 and 20 μm, and the total thickness of the dry film is between 80 and 150 μm.
3. The dry film for electroplating copper pillars according to claim 1, characterized in that: The alkali-soluble resin has a solid content of 40%, a weight average molecular weight of 40,000, and an acid value of 156 mgKOH / g.
4. The dry film for electroplating copper pillars according to claim 1, characterized in that: The mass percentage of the HEMA-IPDI-R-IPDI-HEMA in the photopolymerizable monomer is 30%.
5. The dry film for electroplating copper pillars according to claim 1, characterized in that: The photopolymerizable monomer further includes a vinyl-containing (meth)acrylate compound, and the vinyl-containing (meth)acrylate compound includes one or more of ethoxy nonylphenol (meth)acrylate, propoxy nonylphenol (meth)acrylate, ethoxy bisphenol A di(meth)acrylate, ethoxy di(meth)acrylate, propoxy di(meth)acrylate, ethoxy trimethylolpropane tri(meth)acrylate, and ethoxy pentaerythritol tetra(meth)acrylate.
6. The dry film for electroplating copper pillars according to claim 1, characterized in that: The photoinitiator is a triaryl imidazole dimer derivative, and the photoinitiator includes one or more of 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer, and 2,2',4-tris(2-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenyl-1,1'-diimidazole.
7. The dry film for electroplating copper pillars according to claim 1, characterized in that: The photosensitizer is an anthracene and / or benzophenone compound.
8. The dry film for electroplating copper pillars according to claim 7, characterized in that: The photosensitizer is one or more of 9,10-dibutoxyanthracene, 9,10-dimethoxyanthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-diphenylanthracene, and tetraethyl Michler's ketone.
9. The dry film for electroplating copper pillars according to claim 1, characterized in that: The raw materials of the dry film also include at least one of a light stabilizer, a heat stabilizer, an antioxidant, a photochromic agent, a photoacid generator, a plasticizer, a pigment, a filler, a defoamer, and a leveling agent.
10. An IC carrier copper column, characterized in that: The dry film for electroplating copper columns is prepared from any one of claims 1 to 9.