Bonding process and system of aluminum powder and substrate of anode foil of sintered aluminum electrolytic capacitor

Through the bonding system of the sintered aluminum electrolytic capacitor anode foil aluminum powder and the substrate, the rack and control system are used for intelligent control, which solves the problem of difficulty in ensuring the bonding quality in traditional technology and achieves efficient bonding strength and surface quality.

CN118398385BActive Publication Date: 2024-10-01DONGGUAN AILLEN ELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410589954.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-13
Publication Date
2024-10-01
Estimated Expiration
2044-05-13

AI Technical Summary

Technical Problem

The area expansion rate of traditional aluminum electrolytic capacitor anode foil is close to the limit, the specific capacity growth of the formed foil is stagnant, and the corrosion process produces a large amount of metal ion acidic waste liquid, and it is difficult to ensure that the aluminum powder is evenly mixed and fully bonded to the substrate through binder selection and process design. .

Method used

The bonding system using sintered aluminum electrolytic capacitor anode foil aluminum powder and the substrate includes a frame, raw material mixing assembly, bonding assembly and control system. Through pretreatment, adhesive application, pressing and curing modules, it combines detection and The quality control module realizes intelligent control and full-process supervision to ensure bonding quality.

Benefits of technology

It achieves intelligent control of the capacitor anode foil aluminum powder and the substrate, improves the bonding quality and stability, ensures the bonding strength and surface quality, and avoids the problems of uneven application of the adhesive and incomplete curing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118398385B_ABST
    Figure CN118398385B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of capacitors, and specifically relates to a bonding process and system for aluminum powder of anode foil of a sintered aluminum electrolytic capacitor and a substrate, comprising: a frame, which is used for installing various components; a raw material mixing component, which is arranged on the frame and is used for mixing materials required for bonding aluminum powder of anode of the capacitor and a substrate; a bonding component, which is arranged on the frame and is used for laying raw materials mixed by the raw material mixing component and bonding aluminum powder to the substrate; a control system, which is arranged on the frame and is used for connecting the raw material mixing component and the bonding component and adjusting bonding parameters of aluminum powder and the substrate through the control system and adjusting bonding strategies in real time to complete the production of the foil of the capacitor anode, and has the effect of intelligently controlling the bonding of aluminum powder of the capacitor anode foil and the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of capacitor anode processing, in particular to a bonding process and system for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate. Background Art

[0002] Aluminum electrolytic capacitors are one of the indispensable components in modern electronic products. They have the characteristics of excellent performance, large capacity, low cost, easy processing, and convenient use. They are widely used in important fields such as mobile phones, televisions, household appliances, power supplies, hybrid devices, aerospace, and military, and play the role of filtering, bypassing, coupling, and decoupling in the circuit. Nowadays, most of the anode foils of domestic aluminum electrolytic capacitors use traditional etched foils. However, the expansion rate of traditional etched foils is close to the theoretical limit, the growth of the specific capacity of industrially formed foils is almost stagnant, and the corrosion process will produce a large amount of acidic waste liquid containing metal ions. In recent years, additive manufacturing has been introduced to replace chemical etching. This method uses high-purity aluminum powder and light aluminum foil as the main raw materials. By stacking aluminum powder layers on aluminum foil, the surface undulation of the aluminum powder layer is relied on to increase the specific surface area of ​​the anode foil.

[0003] The technology of preparing electrolytic capacitor anode aluminum foil by coating and sintering aluminum powder slurry is in its infancy in China. Among them, the preparation process of aluminum powder slurry is to evenly mix aluminum powder, solvent, dispersant and binder in a certain proportion, and the selection of binder and the process design of aluminum powder slurry play a vital role in the subsequent sintering and formation. In this process, it is necessary to ensure that the aluminum powder is fully bonded to each other and between the aluminum powder and the aluminum foil substrate, and to ensure that the binder can be easily removed in the subsequent sintering process. Therefore, it is necessary to find a method that can make the aluminum powder be evenly mixed without being damaged, and at the same time can be well bonded to the substrate.

[0004] In view of the above technical defects, a bonding process and system solution for the anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate is proposed. Summary of the invention

[0005] To solve the above problems, the present invention provides the following technical solutions:

[0006] The bonding system of the anode foil aluminum powder and the substrate of the sintered aluminum electrolytic capacitor includes:

[0007] A rack, which is used for installing various components;

[0008] A raw material mixing assembly, the raw material mixing assembly is arranged on the frame, and the raw material mixing assembly is used to mix the aluminum powder of the capacitor anode with the material required for bonding the substrate;

[0009] A bonding component, the bonding component is arranged on the frame, and the bonding component is used to lay the raw materials mixed by the raw material mixing component and bond the aluminum powder to the substrate;

[0010] A control system is provided on the frame, and is used to connect the raw material mixing component with the bonding component and to adjust the bonding parameters of the aluminum powder to the substrate through the control system and to adjust the bonding strategy in real time to complete the production of the capacitor anode foil.

[0011] Furthermore, the raw material mixing assembly includes a mixing box, a stirring rod, a stirring paddle and a driving unit. The mixing box is arranged on the frame, the stirring rod is rotatably connected to the mixing box, the stirring rod and the end inside the mixing box are connected to the stirring paddle, the stirring paddle is used to mix and stir the raw materials in the mixing box, and the driving unit is connected to the stirring rod to drive the stirring rod to rotate.

[0012] Furthermore, the bonding assembly includes a bonding plate, a storage plate, and a driving rod. The storage plate is arranged on the frame, the bonding plate is arranged to be raised and lowered along the frame, the driving rod is arranged on the frame, the driving rod is connected to the bonding plate, and the driving rod is used to drive the bonding plate to move along the frame and drive the capacitor anode foil aluminum powder to be bonded and fixed to the substrate.

[0013] Furthermore, the control system comprises:

[0014] Pre-treatment module: used to treat the anode foil aluminum powder and substrate, clean the surface, remove impurities before bonding, and possibly perform surface treatment to improve bonding performance;

[0015] Adhesive application module: used to apply adhesive to the anode foil aluminum powder or substrate surface. The selection and application method of adhesive will directly affect the bonding quality;

[0016] Lamination module: After the adhesive is applied, the anode foil aluminum powder and the substrate are pressed together to ensure good bonding, and is responsible for applying appropriate pressure and temperature to achieve effective bonding;

[0017] Curing module: Curing of the adhesive can ensure stable bonding. The curing module provides appropriate conditions, such as temperature and time, to cure the adhesive;

[0018] Inspection and quality control module: The system uses the inspection and quality control module to detect indicators such as bonding strength and surface quality, and to make necessary adjustments and controls.

[0019] Furthermore, the preprocessing module includes:

[0020] Clean the surface: By cleaning the surface, remove impurities, oil stains and other pollutants on the surface to ensure that the bonding surface is clean and smooth, which is conducive to the adhesion of the adhesive and the improvement of the bonding quality;

[0021] Removing the oxide layer: Aluminum materials form an oxide layer in the air, which affects the quality of bonding. The pretreatment module includes a process for removing the oxide layer to ensure that the surface of the anode foil aluminum powder and the substrate is a fresh metal surface;

[0022] Surface treatment: The pretreatment module performs surface treatment on the anode foil aluminum powder and the substrate, such as sandblasting and chemical treatment, to increase the surface roughness and enhance the surface activity, thereby improving the adhesion and bonding strength of the adhesive;

[0023] Adjusting surface energy: The surface energy of the anode foil aluminum powder and the substrate is adjusted through the pretreatment module, so that the anode foil aluminum powder and the substrate interact better with the adhesive, thereby improving the stability and reliability of the bonding.

[0024] Furthermore, the adhesive applying module comprises:

[0025] Adhesive selection: Select a suitable adhesive according to its properties and process requirements. The adhesive is a material with good adhesion, high temperature stability and chemical stability;

[0026] Adhesive application method: Determine the appropriate adhesive application method, such as spraying, coating, and rolling, to ensure that the adhesive can evenly cover the surface of the anode foil aluminum powder or the substrate, and the amount and thickness of the adhesive can meet the requirements of bonding quality;

[0027] Adhesive curing pretreatment: After the adhesive is applied, some pretreatment work is required, such as waiting for a certain period of time for the adhesive to penetrate the surface, or using hot air or ultraviolet rays to promote the curing and adhesion of the adhesive;

[0028] Adhesive application control: Monitor and control the adhesive application process to ensure the quality and stability of adhesive application, which involves the adjustment and control of adhesive flow, application speed, and application pressure parameters.

[0029] Furthermore, the detection and quality control module includes:

[0030] Bond strength test: Use appropriate test methods, such as stretching and shearing, to test the strength of the bonded parts to ensure the firmness and stability of the bond;

[0031] Surface quality inspection: inspect the surface quality of the bonding parts, including surface flatness, surface cleanliness, and oxide layer conditions, to ensure that the surface conditions meet the requirements and do not affect the bonding quality;

[0032] Adhesive curing quality inspection: inspect the quality of the adhesive after curing, including the curing degree and curing uniformity indicators, to ensure the completeness and stability of the adhesive curing;

[0033] Bonding process parameter monitoring: monitor key parameters in the bonding process, such as temperature, pressure, and time, to ensure the stability and controllability of the bonding process and avoid affecting the bonding quality due to parameter fluctuations;

[0034] Abnormality detection and handling: Detect and handle abnormalities that occur during the bonding process, such as uneven application of adhesive and incomplete curing, to prevent these abnormalities from affecting the quality of the final product.

[0035] According to another aspect of the present invention, there is provided a bonding process for the bonding system of the anode foil aluminum powder of the sintered aluminum electrolytic capacitor and the substrate, comprising the following steps:

[0036] Step 1: Slurry preparation: spherical aluminum powder, binder, organic solvent and dispersant are mixed evenly in a certain mass ratio to form aluminum powder slurry;

[0037] Step 2: coating, uniformly coating the mixed aluminum powder slurry obtained in step 1 on both sides of the aluminum foil substrate to form a slurry layer;

[0038] Step 3: Drying: placing the aluminum foil with the aluminum slurry layer after coating in step 2 in a vacuum dryer for drying to obtain a dried coated aluminum foil;

[0039] Step 4: sintering: sintering the dried coated aluminum foil obtained in step 3 at a temperature of 560-660° C. for 5-600 min.

[0040] Furthermore, in step 1, the binder in the aluminum powder slurry for the anode foil of the sintered aluminum electrolytic capacitor is a mixed binder;

[0041] The particle size of the spherical aluminum powder is 1-5 μm; the solvent is one or more of deionized water, ethanol, ethylene glycol or pinene alcohol; the binder is one or more of carboxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinylidene fluoride or phenolic resin; the dispersant is one or more of oleic acid, polyvinyl alcohol, stearic acid or glycerol.

[0042] Furthermore, in step 1, the aluminum powder slurry further comprises a solvent, a binder and a dispersant, and the weight ratio of the aluminum powder particles, the solvent, the binder and the dispersant is (55-70): (25-40): (1-4): (1-4);

[0043] The purity of the aluminum powder particles is greater than 99.98%.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] 1. In the bonding process and system of the anode foil aluminum powder of the sintered aluminum electrolytic capacitor and the substrate of the present invention, a rack is used to install various components; a raw material mixing component is arranged on the rack, and the raw material mixing component is used to mix the materials required for bonding the aluminum powder of the capacitor anode and the substrate; a bonding component is arranged on the rack, and the bonding component is used to lay the raw materials mixed by the raw material mixing component and bond the aluminum powder to the substrate; a control system is arranged on the rack, and the control system is used to connect the raw material mixing component and the bonding component and adjust the bonding parameters of the aluminum powder to the substrate through the control system and adjust the bonding strategy in real time to complete the production of the capacitor anode foil, which has the effect of intelligently controlling the bonding of the capacitor anode foil aluminum powder and the substrate;

[0046] 2. In the bonding process and system of the anode foil aluminum powder and the substrate of the sintered aluminum electrolytic capacitor of the present invention, a pretreatment module is used to treat the anode foil aluminum powder and the substrate, clean the surface and remove impurities before bonding, and may perform surface treatment to improve the bonding performance; an adhesive application module is used to apply the adhesive to the surface of the anode foil aluminum powder or the substrate, and the selection and application method of the adhesive will directly affect the bonding quality; a pressing module: after the adhesive is applied, the anode foil aluminum powder and the substrate are pressed to ensure good bonding, and the module is responsible for applying appropriate pressure and temperature to achieve effective bonding; a curing module: the adhesive is cured to ensure stable bonding, and the curing module provides appropriate conditions, such as temperature and time, to cure the adhesive; a detection and quality control module: the system is used to detect indicators such as bonding strength and surface quality, and to make necessary adjustments and controls through the detection and quality control module, which has the effect of supervising the entire process of the bonding process and system of the capacitor anode foil aluminum powder and the substrate and adjusting the bonding strategy in real time to ensure stable bonding. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to facilitate understanding by those skilled in the art, the present invention is further described below in conjunction with the accompanying drawings;

[0048] Figure 1 The overall structural schematic diagram of the bonding system of the anode foil aluminum powder and the substrate of the sintered aluminum electrolytic capacitor of the present invention;

[0049] Figure 2 It is a structural schematic diagram of a raw material mixing assembly in a bonding system of aluminum powder of anode foil and substrate of a sintered aluminum electrolytic capacitor of the present invention;

[0050] Figure 3 It is a schematic diagram of the bonding process of the anode foil aluminum powder of the sintered aluminum electrolytic capacitor and the substrate of the present invention;

[0051] Figure 4This is a scanning electron microscope image of the coated foil produced in Example 1;

[0052] Figure 5 This is a scanning electron microscope image of the coated foil produced in Example 2;

[0053] Figure 6 Scanning electron microscope images of the coated foils produced for Comparative Examples 1, 2, 3 and 4;

[0054] Figure 7 This is a physical picture of the coated aluminum foil and sintered foil produced in Comparative Example 1.

[0055] Figure numerals: 1, frame; 2, raw material mixing assembly; 21, mixing box; 22, stirring rod; 23, stirring paddle; 3, bonding assembly; 31, bonding plate; 32, storage plate; 33, driving rod. DETAILED DESCRIPTION

[0056] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0057] like Figure 1-Figure 7 As shown, the bonding process and system of aluminum powder of anode foil of sintered aluminum electrolytic capacitor and substrate include: a frame 1, which is used for installing various components; a raw material mixing component 2, which is arranged on the frame 1, and is used for mixing materials required for bonding aluminum powder of capacitor anode and substrate; a bonding component 3, which is arranged on the frame 1, and is used for laying raw materials mixed by the raw material mixing component 2 and bonding aluminum powder to the substrate; a control system, which is arranged on the frame 1, and is used for connecting the raw material mixing component 2 and the bonding component 3 and adjusting the bonding parameters of aluminum powder to the substrate and adjusting the bonding strategy in real time through the control system to complete the production of capacitor anode foil.

[0058] Specifically, the raw material mixing assembly 2 includes a mixing box 21, a stirring rod 22, a stirring paddle 23 and a driving unit. The mixing box 21 is arranged on the frame 1. The stirring rod 22 is rotatably connected to the mixing box 21. The end of the stirring rod 22 in the mixing box 21 is connected to the stirring paddle 23. The stirring paddle 23 is used to mix and stir the raw materials in the mixing box 21. The driving unit is connected to the stirring rod 22 to drive the stirring rod 22 to rotate. The bonding assembly 3 includes a bonding plate 31, a storage plate 32, and a driving rod 33. The storage plate 32 is arranged on the frame 1. The bonding plate 31 is arranged to be lifted and lowered along the frame 1. The driving rod 33 is arranged on the frame 1. The driving rod 33 is connected to the bonding plate 31. The driving rod 33 is used to drive the bonding plate 31 to move along the frame 1 and drive the capacitor anode foil aluminum powder to be bonded and fixed to the substrate, which has the effect of intelligently controlling the bonding of the capacitor anode foil aluminum powder and the substrate.

[0059] Specifically, the control system includes:

[0060] Pre-treatment module: used to treat the anode foil aluminum powder and substrate, clean the surface, remove impurities before bonding, and possibly perform surface treatment to improve bonding performance;

[0061] Adhesive application module: used to apply adhesive to the anode foil aluminum powder or substrate surface. The selection and application method of adhesive will directly affect the bonding quality;

[0062] Lamination module: After the adhesive is applied, the anode foil aluminum powder and the substrate are pressed together to ensure good bonding, and is responsible for applying appropriate pressure and temperature to achieve effective bonding;

[0063] Curing module: Curing of the adhesive can ensure stable bonding. The curing module provides appropriate conditions, such as temperature and time, to cure the adhesive;

[0064] Inspection and quality control module: The system uses the inspection and quality control module to detect indicators such as bonding strength and surface quality, and to make necessary adjustments and controls.

[0065] Specifically, the preprocessing module includes:

[0066] Clean the surface: By cleaning the surface, remove impurities, oil stains and other pollutants on the surface to ensure that the bonding surface is clean and smooth, which is conducive to the adhesion of the adhesive and the improvement of the bonding quality;

[0067] Removing the oxide layer: Aluminum materials form an oxide layer in the air, which affects the quality of bonding. The pretreatment module includes a process for removing the oxide layer to ensure that the surface of the anode foil aluminum powder and the substrate is a fresh metal surface;

[0068] Surface treatment: The pretreatment module performs surface treatment on the anode foil aluminum powder and the substrate, such as sandblasting and chemical treatment, to increase the surface roughness and enhance the surface activity, thereby improving the adhesion and bonding strength of the adhesive;

[0069] Adjusting surface energy: The surface energy of the anode foil aluminum powder and the substrate is adjusted through the pretreatment module, so that the anode foil aluminum powder and the substrate interact better with the adhesive, thereby improving the stability and reliability of the bonding.

[0070] Specifically, the adhesive applying module includes:

[0071] Adhesive selection: Select a suitable adhesive according to its properties and process requirements. The adhesive is a material with good adhesion, high temperature stability and chemical stability;

[0072] Adhesive application method: Determine the appropriate adhesive application method, such as spraying, coating, and rolling, to ensure that the adhesive can evenly cover the surface of the anode foil aluminum powder or the substrate, and the amount and thickness of the adhesive can meet the requirements of bonding quality;

[0073] Adhesive curing pretreatment: After the adhesive is applied, some pretreatment work is required, such as waiting for a certain period of time for the adhesive to penetrate the surface, or using hot air or ultraviolet rays to promote the curing and adhesion of the adhesive;

[0074] Adhesive application control: Monitor and control the adhesive application process to ensure the quality and stability of adhesive application, which involves the adjustment and control of adhesive flow, application speed, and application pressure parameters.

[0075] Specifically, the detection and quality control module includes:

[0076] Bond strength test: Use appropriate test methods, such as stretching and shearing, to test the strength of the bonded parts to ensure the firmness and stability of the bond;

[0077] Surface quality inspection: inspect the surface quality of the bonding parts, including surface flatness, surface cleanliness, and oxide layer conditions, to ensure that the surface conditions meet the requirements and do not affect the bonding quality;

[0078] Adhesive curing quality inspection: inspect the quality of the adhesive after curing, including the curing degree and curing uniformity indicators, to ensure the completeness and stability of the adhesive curing;

[0079] Bonding process parameter monitoring: monitor key parameters in the bonding process, such as temperature, pressure, and time, to ensure the stability and controllability of the bonding process and avoid affecting the bonding quality due to parameter fluctuations;

[0080] Abnormality detection and handling: Detect and handle abnormalities that occur during the bonding process, such as uneven application of adhesive and incomplete curing, to prevent these abnormalities from affecting the quality of the final product.

[0081] Specifically, when controlling the bonding between the container anode foil aluminum powder and the substrate, the PID algorithm is used to control the output and input, including building a PID algorithm to adjust the control system in real time, as follows:

[0082]

[0083] Among them, u(k) is the controller output, K p is the proportionality coefficient, K i is the integration coefficient, K d is the differential coefficient, e(k) is the proportional output, e(n) is the integral output, and e(k)-e(k-1) is the differential output. The PID control algorithm is used to monitor the raw material mixing components and bonding components on the rack, and the control loop on the rack is monitored for safety status and real-time feedback, ensuring that the bonding process of the capacitor anode foil aluminum powder and the substrate is fully controlled and the bonding strategy is adjusted in real time.

[0084] The control loop and the loop parameters of the raw material mixing component and the bonding component are monitored by setting sensors on the rack, and the collected data are cleaned, screened and visualized for analysis. The data visualization includes image processing, and the image processing includes image scaling. The pixels of the image are adjusted by building a convolutional neural network. The neurons in each layer of the convolutional neural network are arranged in three dimensions: width, height and depth. For the input layer, the width and height refer to the width and height of the input image, and the depth represents the number of channels of the input image, which is calculated by the following formula:

[0085]

[0086] Among them, n out is the output size, n in is the input size, p is the padding size, f is the convolution kernel size, s is the convolution step size. The original image is scaled by combining the pixel input size of the original image with the padding size through the convolution neural network, and the width, height and depth of the original image are modified. After the original image is scaled, the clarity of the original image is guaranteed, so as to visualize the whole process of the bonding process between the capacitor anode foil aluminum powder and the substrate, judge the bonding situation according to the displayed situation, and then adjust the bonding strategy.

[0087] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0088] 1) Slurry preparation: spherical aluminum powder, binder, organic solvent and dispersant are mixed uniformly in a certain mass ratio to form aluminum powder slurry;

[0089] In the present invention, the spherical aluminum powder particles selected need to be as uniform as possible, because small particles of powder will fill the gaps formed between large particles of powder, thereby affecting the porosity of the sintered film after sintering; the selected adhesive must be compatible with the type and properties of the bonded material, and must also meet the requirements of the mechanical and physical properties of the bonded joint. Finally, the feasibility, economy, and balance of performance and cost of the bonding process must also be considered.

[0090] 2) coating, uniformly coating the mixed aluminum powder slurry obtained in step 1) on both sides of the aluminum foil substrate to form a slurry layer;

[0091] 3) drying, placing the aluminum foil with the aluminum slurry layer after coating in step 2) in a vacuum dryer for drying to obtain a dried coated aluminum foil;

[0092] During the ball milling process, the ball milling speed and ball milling time should be correctly selected to ensure that the aluminum powder particles can be evenly mixed and to avoid the aluminum powder particles being damaged by excessive ball milling. 4) Sintering: The dried coated aluminum foil obtained in step 3) is sintered at a temperature of 560-660°C for 5-600 minutes to form sintering necks between the aluminum powders and between the aluminum powders and the aluminum foil substrate. The purpose of sintering is to remove excess binder and melt the aluminum powder particles to form interconnected sintering necks.

[0093] Embodiment 1:

[0094] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0095] 1) Slurry configuration:

[0096] High-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, carboxymethyl cellulose and ethylene glycol were mixed in a weight ratio of 55:4:1:40, and then the mixed raw materials were put into a ball mill and ball-milled at a speed of 300 rpm to obtain a slurry:

[0097] 2) Coating:

[0098] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate with a coating thickness of 150-300 μm to form a slurry layer;

[0099] 3) Drying:

[0100] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0101] 4) Sintering: sintering the dried coated aluminum foil obtained in step 3) at a temperature of 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate.

[0102] Morphology detection: The microscopic morphology of the coated aluminum foil and the sintered foil was analyzed using a scanning electron microscope.

[0103] Embodiment 2:

[0104] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0105] 1) Slurry configuration:

[0106] High-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, phenolic resin and ethylene glycol were mixed in a weight ratio of 55:4:1:40, and then the mixed raw materials were put into a ball mill and ball-milled at a speed of 300 rpm to obtain a slurry:

[0107] 2) Coating:

[0108] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate, with a coating thickness of 150-300 μm to form a slurry layer; 3) Drying:

[0109] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0110] 4) Sintering: sinter the dried coated aluminum foil obtained in step 3) at 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate. Morphology detection: The microscopic morphology of the coated aluminum foil and the sintered foil is analyzed using a scanning electron microscope.

[0111] Comparative Example 1:

[0112] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0113] 1) Slurry configuration:

[0114] High-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, a binder (carboxymethyl cellulose and phenolic resin in a weight ratio of 1:1) and ethylene glycol were mixed in a weight ratio of 55:4:1:40, and then the mixed raw materials were put into a ball mill and ball-milled at a speed of 300 rpm to obtain a slurry:

[0115] 2) Coating:

[0116] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate with a coating thickness of 150-300 μm to form a slurry layer;

[0117] 3) Drying:

[0118] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0119] 4) Sintering: sinter the dried coated aluminum foil obtained in step 3) at 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate. Morphology detection: The microscopic morphology of the coated aluminum foil and the sintered foil is analyzed using a scanning electron microscope.

[0120] This comparative example is basically the same as Example 1, with the only difference being that high-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, a binder (carboxymethyl cellulose and phenolic resin in a weight ratio of 1:1) and ethylene glycol are mixed in a weight ratio of 55:4:1:40, and then the above raw materials are mixed and put into a ball mill, and ball milled at a rotation speed of 300 rpm to obtain a slurry. The type of binder in this comparative example is different.

[0121] Comparative Example 2:

[0122] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0123] 1) Slurry configuration:

[0124] High-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, a binder (carboxymethyl cellulose and phenolic resin in a weight ratio of 3:2) and ethylene glycol were mixed in a weight ratio of 55:4:1:40, and then the mixed raw materials were put into a ball mill and ball-milled at a speed of 300 rpm to obtain a slurry:

[0125] 2) Coating:

[0126] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate with a coating thickness of 150-300 μm to form a slurry layer;

[0127] 3) Drying:

[0128] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0129] 5) Sintering: sinter the dried coated aluminum foil obtained in step 3) at 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate. Morphology detection: The microscopic morphology of the coated aluminum foil and the sintered foil is analyzed using a scanning electron microscope.

[0130] This comparative example is basically the same as Example 1, with the only difference being that high-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, a binder (carboxymethyl cellulose and phenolic resin in a weight ratio of 3:2) and ethylene glycol are mixed in a weight ratio of 55:4:1:40, and then the above raw materials are mixed and put into a ball mill, and ball milled at a rotation speed of 300 rpm to obtain a slurry. The type of binder in this comparative example is different.

[0131] Comparative Example 3:

[0132] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0133] 1) Slurry configuration:

[0134] High-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, a binder (carboxymethyl cellulose and phenolic resin in a weight ratio of 7:3) and ethylene glycol were mixed in a weight ratio of 55:4:1:40, and then the mixed raw materials were put into a ball mill and ball-milled at a speed of 300 rpm to obtain a slurry:

[0135] 2) Coating:

[0136] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate with a coating thickness of 150-300 μm to form a slurry layer;

[0137] 3) Drying:

[0138] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0139] 4) Sintering: sinter the dried coated aluminum foil obtained in step 3) at 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate. Morphology detection: The microscopic morphology of the coated aluminum foil and the sintered foil is analyzed using a scanning electron microscope.

[0140] This comparative example is basically the same as Example 1, with the only difference being that high-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, a binder (carboxymethyl cellulose and phenolic resin in a weight ratio of 7:3) and ethylene glycol are mixed in a weight ratio of 55:4:1:40, and then the above raw materials are mixed and put into a ball mill, and ball milled at a rotation speed of 300 rpm to obtain a slurry. The type of binder in this comparative example is different.

[0141] Comparative Example 4:

[0142] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0143] 1) Slurry preparation: High-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, a binder (carboxymethyl cellulose and phenolic resin in a weight ratio of 8:2) and ethylene glycol are mixed in a weight ratio of 55:4:1:40, and then the above raw materials are mixed and put into a ball mill and ball milled at a speed of 300 rpm to obtain a slurry:

[0144] 2) Coating:

[0145] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate with a coating thickness of 150-300 μm to form a slurry layer;

[0146] 3) Drying:

[0147] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0148] 5) Sintering: sinter the dried coated aluminum foil obtained in step 3) at 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate. Morphology detection: The microscopic morphology of the coated aluminum foil and the sintered foil is analyzed using a scanning electron microscope.

[0149] This comparative example is basically the same as Example 1, with the only difference being that high-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, a binder (carboxymethyl cellulose and phenolic resin in a weight ratio of 8:2) and ethylene glycol are mixed in a weight ratio of 55:4:1:40, and then the above raw materials are mixed and put into a ball mill, and ball milled at a rotation speed of 300 rpm to obtain a slurry. The type of binder in this comparative example is different.

[0150] Comparative Example 5:

[0151] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0152] 1) Slurry configuration:

[0153] High-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, polyvinylidene fluoride and ethylene glycol were mixed in a weight ratio of 55:4:1:40, and then the mixed raw materials were put into a ball mill and ball-milled at a speed of 300 rpm to obtain a slurry:

[0154] 2) Coating:

[0155] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate with a coating thickness of 150-300 μm to form a slurry layer;

[0156] 3) Drying:

[0157] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0158] 4) Sintering: sinter the dried coated aluminum foil obtained in step 3) at 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate. Morphology detection: The microscopic morphology of the coated aluminum foil and the sintered foil is analyzed using a scanning electron microscope.

[0159] This comparative example is basically the same as Example 1, with the only difference being that high-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, polyvinylidene fluoride and ethylene glycol are mixed in a weight ratio of 55:4:1:40, and then the above raw materials are mixed and put into a ball mill, and ball milled at a rotation speed of 300 rpm to obtain a slurry. The types of adhesives in this comparative example are different.

[0160] Comparative Example 6:

[0161] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0162] 1) Slurry configuration:

[0163] High-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, polyvinyl alcohol and ethylene glycol were mixed in a weight ratio of 55:4:1:40, and then the mixed raw materials were put into a ball mill and ball-milled at a speed of 300 rpm to obtain a slurry:

[0164] 2) Coating:

[0165] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate with a coating thickness of 150-300 μm to form a slurry layer;

[0166] 3) Drying:

[0167] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0168] 5) Sintering: sintering the dried coated aluminum foil obtained in step 3) at a temperature of 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate.

[0169] This comparative example is basically the same as Example 1, with the only difference being that high-purity aluminum powder with an average particle size of 3-5 μm, oleic acid, polyvinyl alcohol and ethylene glycol are mixed in a weight ratio of 55:4:1:40, and then the above raw materials are mixed and put into a ball mill, and ball milled at a rotation speed of 300 rpm to obtain a slurry. The types of adhesives in this comparative example are different.

[0170] Comparative Example 7:

[0171] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0172] 1) Slurry configuration:

[0173] High-purity aluminum powder with an average particle size of 3-5 μm, triethanolamine, dibutyl phthalate, polyvinyl butyral and anhydrous ethanol were mixed in a weight ratio of 55:1:1:3:40, and then the mixed raw materials were put into a ball mill and ball-milled at a speed of 300 rpm to obtain a slurry:

[0174] 2) Coating:

[0175] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate with a coating thickness of 150-300 μm to form a slurry layer;

[0176] 3) Drying:

[0177] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0178] 4) Sintering: sinter the dried coated aluminum foil obtained in step 3) at 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate. Morphology detection: The microscopic morphology of the coated aluminum foil and the sintered foil is analyzed using a scanning electron microscope.

[0179] This comparative example is basically the same as Example 1, except that high-purity aluminum powder with an average particle size of 3-5 μm, triethanolamine, dibutyl phthalate, polyvinyl butyral and anhydrous ethanol are mixed in a weight ratio of 55:1:1:3:40, and then the above raw materials are mixed and put into a ball mill, and ball milled at a rotation speed of 300 rpm to obtain a slurry. The types of adhesives in this comparative example are different.

[0180] Comparative Example 8:

[0181] A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate comprises the following steps:

[0182] 1) Slurry configuration:

[0183] High-purity aluminum powder with an average particle size of 3-5 μm, triethanolamine, dibutyl phthalate, polyvinyl butyral and anhydrous ethanol were mixed in a weight ratio of 60:1:1:3:35, and then the mixed raw materials were put into a ball mill and ball-milled at a speed of 300 rpm to obtain a slurry:

[0184] 2) Coating:

[0185] The mixed aluminum powder slurry obtained in step 1) is evenly coated on both sides of the aluminum foil substrate with a coating thickness of 150-300 μm to form a slurry layer;

[0186] 3) Drying:

[0187] The aluminum foil with the aluminum slurry layer after coating in step 2) is vacuum dried at 80° C. for 12 hours to obtain a dried coated aluminum foil;

[0188] 4) Sintering: sinter the dried coated aluminum foil obtained in step 3) at 560-660° C. for 5-600 min in an argon environment, so that sintering necks are formed between the aluminum powders and between the aluminum powders and the aluminum foil substrate. Morphology detection: The microscopic morphology of the coated aluminum foil and the sintered foil is analyzed using a scanning electron microscope.

[0189] This comparative example is basically the same as Example 1, except that high-purity aluminum powder with an average particle size of 3-5 μm, triethanolamine, dibutyl phthalate, polyvinyl butyral and anhydrous ethanol are mixed in a weight ratio of 60:1:1:3:35, and then the above raw materials are mixed and put into a ball mill, and ball milled at a rotation speed of 300 rpm to obtain a slurry. The types of adhesives in this comparative example are different.

[0190] The working principle of the bonding process and system of the anode foil aluminum powder of the sintered aluminum electrolytic capacitor and the substrate of the present invention is as follows: a frame is used for installing various components; a raw material mixing component is arranged on the frame, and the raw material mixing component is used to mix materials required for bonding the aluminum powder of the capacitor anode and the substrate; a bonding component is arranged on the frame, and the bonding component is used to lay the raw materials mixed by the raw material mixing component and bond the aluminum powder to the substrate; a control system is arranged on the frame, and the control system is used to connect the raw material mixing component and the bonding component and adjust the bonding parameters of the aluminum powder to the substrate and adjust the bonding strategy in real time through the control system to complete the production of the capacitor anode foil, which has the effect of intelligently controlling the bonding of the capacitor anode foil aluminum powder and the substrate; a pretreatment module is used to process the anode foil aluminum powder and the substrate, clean the surface and remove impurities before bonding, and can Surface treatment can be performed to improve bonding performance; Adhesive application module: used to apply adhesive to the surface of the anode foil aluminum powder or the substrate. The selection and application method of the adhesive will directly affect the bonding quality; Pressing module: After the adhesive is applied, the anode foil aluminum powder and the substrate are pressed to ensure good bonding, and it is responsible for applying appropriate pressure and temperature to achieve effective bonding; Curing module: The adhesive must be cured to ensure stable bonding. The curing module provides appropriate conditions, such as temperature and time, to cure the adhesive; Detection and quality control module: The system uses the detection and quality control module to detect indicators such as bonding strength and surface quality, as well as to make necessary adjustments and controls. It has the effect of supervising the entire process of the bonding process and system of the capacitor anode foil aluminum powder and the substrate, and adjusting the bonding strategy in real time to ensure stable bonding.

[0191] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A bonding system for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate, characterized in that: include: A rack (1), wherein the rack (1) is used for installing various components; A raw material mixing assembly (2), the raw material mixing assembly (2) being arranged on the frame (1), the raw material mixing assembly (2) being used to mix aluminum powder of a capacitor anode with materials required for bonding with a substrate, the raw material mixing assembly (2) comprising a mixing box (21), a stirring rod (22), a stirring paddle (23) and a driving unit, the mixing box (21) being arranged on the frame (1), the stirring rod (22) being rotatably connected to the mixing box (21), the end of the stirring rod (22) in the mixing box (21) being connected to the stirring paddle (23), the stirring paddle (23) being used to mix and stir the raw materials in the mixing box (21), and the driving unit being connected to the stirring rod (22) and being used to drive the stirring rod (22) to rotate; A bonding component (3), the bonding component (3) being arranged on the frame (1), the bonding component (3) being used to lay the raw materials mixed by the raw material mixing component (2) and to bond the aluminum powder to the substrate, the bonding component (3) comprising a bonding plate (31), a storage plate (32), and a driving rod (33), the storage plate (32) being arranged on the frame (1), the bonding plate (31) being arranged to be lifted and lowered along the frame (1), the driving rod (33) being arranged on the frame (1), the driving rod (33) being connected to the bonding plate (31), and the driving rod (33) being used to drive the bonding plate (31) to move along the frame (1) and drive the capacitor anode foil aluminum powder to be bonded and fixed to the substrate; A control system is provided on the frame (1), the control system is used to connect the raw material mixing component (2) and the bonding component (3) and to adjust the bonding parameters between the aluminum powder and the substrate and the bonding strategy in real time through the control system to complete the production of the capacitor anode foil.

2. The bonding system of sintered aluminum electrolytic capacitor anode foil aluminum powder and substrate according to claim 1, characterized in that: The control system comprises: Pretreatment module: used to process the anode foil aluminum powder and substrate, clean the surface, remove impurities before bonding, and perform surface treatment to improve bonding performance; Adhesive application module: used to apply adhesive to the anode foil aluminum powder or substrate surface. The selection and application method of adhesive will directly affect the bonding quality; Lamination module: After the adhesive is applied, the anode foil aluminum powder and the substrate are pressed together to ensure good bonding, and is responsible for applying appropriate pressure and temperature to achieve effective bonding; Curing module: Curing of the adhesive can ensure stable bonding. The curing module provides appropriate temperature and time to cure the adhesive; Inspection and quality control module: The system uses the inspection and quality control module to detect bonding strength, surface quality, and make adjustments and controls.

3. The bonding system of sintered aluminum electrolytic capacitor anode foil aluminum powder and substrate according to claim 2, characterized in that: The preprocessing module comprises: Clean the surface: By cleaning the surface, remove impurities and oil stains on the surface to ensure that the bonding surface is clean and smooth, which is conducive to the adhesion of the adhesive and the improvement of the bonding quality; Removing the oxide layer: Aluminum materials form an oxide layer in the air, which affects the quality of bonding. The oxide layer removal process is implemented through the pretreatment module to ensure that the surface of the anode foil aluminum powder and the substrate is a fresh metal surface; Surface treatment: The pretreatment module performs surface treatment on the anode foil aluminum powder and the substrate, and the surface treatment includes sandblasting and chemical treatment to increase the surface roughness and enhance the surface activity, thereby improving the adhesion and bonding strength of the adhesive; Adjusting surface energy: The surface energy of the anode foil aluminum powder and the substrate is adjusted through the pretreatment module, so that the anode foil aluminum powder and the substrate interact better with the adhesive, thereby improving the stability and reliability of the bonding.

4. The bonding system of sintered aluminum electrolytic capacitor anode foil aluminum powder and substrate according to claim 3, characterized in that: The adhesive application module comprises: Adhesive selection: Select the appropriate adhesive according to its properties and process requirements; Adhesive application method: Determine the appropriate adhesive application method, which includes spraying and rolling, to ensure that the adhesive can evenly cover the surface of the anode foil aluminum powder or the substrate, and the amount and thickness of the adhesive can meet the requirements of bonding quality; Adhesive curing pretreatment: After the adhesive is applied, some pretreatment work is required, which includes waiting for a certain period of time for the adhesive to penetrate the surface, or using hot air or ultraviolet rays to promote the curing and adhesion of the adhesive; Adhesive application control: Monitor and control the adhesive application process to ensure the quality and stability of adhesive application, which involves the adjustment and control of adhesive flow, application speed, and application pressure parameters.

5. The bonding system of sintered aluminum electrolytic capacitor anode foil aluminum powder and substrate according to claim 4, characterized in that: The detection and quality control module includes: Bond strength test: Use appropriate test methods, including stretching and shearing, to test the strength of the bonded parts to ensure the firmness and stability of the bond; Surface quality inspection: inspect the surface quality of the bonding parts, including surface flatness, surface cleanliness, and oxide layer conditions, to ensure that the surface conditions meet the requirements and do not affect the bonding quality; Adhesive curing quality inspection: inspect the quality of the adhesive after curing, including the curing degree and curing uniformity indicators, to ensure the completeness and stability of the adhesive curing; Bonding process parameter monitoring: monitor key parameters in the bonding process, including temperature, pressure, and time, to ensure the stability and controllability of the bonding process and avoid affecting the bonding quality due to parameter fluctuations; Abnormality detection and processing: Detect and handle abnormalities that occur during the bonding process, such as uneven application of adhesive and incomplete curing, to prevent these abnormalities from affecting the quality of the final product.

6. A bonding process for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate, the bonding system for anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: Slurry preparation: spherical aluminum powder, binder, organic solvent and dispersant are mixed evenly in a certain mass ratio to form aluminum powder slurry; Step 2: coating, evenly bonding the mixed aluminum powder slurry obtained in step 1 to the front and back sides of the aluminum foil substrate to form a slurry layer; Step 3: Drying: placing the aluminum foil with the aluminum slurry layer after bonding in step 2 in a vacuum dryer for drying to obtain a dried aluminum foil; Step 4: sintering: sinter the dried aluminum foil obtained in step 3 at a temperature of 560-660° C. for 5-600 min.

7. The bonding process of the anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate according to claim 6, characterized in that: In the step 1, the binder in the aluminum powder slurry for the anode foil of the sintered aluminum electrolytic capacitor is a mixed binder; The particle size of the spherical aluminum powder is 1-5 μm; the solvent is one or more of deionized water, ethanol, ethylene glycol or pinene alcohol; the binder is one or more of carboxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinylidene fluoride or phenolic resin; the dispersant is one or more of oleic acid, polyvinyl alcohol, stearic acid or glycerol.

8. The bonding process of the anode foil aluminum powder of a sintered aluminum electrolytic capacitor and a substrate according to claim 7, characterized in that: In the step 1, the weight ratio of the spherical aluminum powder, the solvent, the binder and the dispersant is (55-70): (25-40): (1-4): (1-4); The purity of the spherical aluminum powder is greater than 99.98%.