A fuse active triggering structure and its preparation process

By printing resistor paste on the ceramic substrate, a high-resistance fuse active triggering structure is formed, which solves the problem of passive blowing of existing fuses, achieves rapid response and circuit protection under abnormal conditions, and avoids additional damage.

CN118398455BActive Publication Date: 2024-10-29ZHUHAI 4U ELECTRONICS CERAMICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410834031.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Existing fuses can only be passively blown in the circuit and cannot detect abnormal conditions in advance, resulting in the inability to effectively protect the circuit. After triggering, the high temperature will cause the carrier to collapse, causing additional damage.

Method used

Design an active triggering structure of a fuse, using a combination of ceramic substrate and resistor slurry. By setting positive electrodes, negative electrodes and connecting contacts on the ceramic substrate, and adding tungsten powder and porcelain powder to the resistor slurry, they are printed and burned on the ceramic substrate. on, forming a high resistance value to quickly fuse under abnormal conditions.

Benefits of technology

It achieves rapid response under abnormal conditions to avoid loss spread, and quickly fuses after detecting an abnormality to protect the circuit without damaging the carrier.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118398455B_ABST
    Figure CN118398455B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of fuse auxiliary technology, and specifically to a fuse active triggering structure and its preparation process, including a ceramic substrate, a resistor paste printed and burned in the ceramic substrate, a positive electrode arranged on one side of the ceramic substrate and connected to one end of the resistor paste, a negative electrode arranged on the other side of the ceramic substrate and connected to the other end of the resistor paste, and connecting contacts arranged on both sides of the positive electrode and the negative electrode, wherein the ceramic substrate is divided into a positive plate and a negative plate in sequence along its thickness direction, the positive plate and the negative plate are bonded by hot pressing, and the resistor paste is printed and burned on the bonding surface of the positive plate and the negative plate. The problem that the existing fuse can only be blown passively and cannot detect abnormalities in advance and blown, thereby better protecting the entire circuit, is effectively solved; the present invention can instantly generate a large current and generate a large amount of heat in a short time, so that the fuse can be blown more quickly to avoid causing additional losses.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of fuse auxiliary technology, and in particular to a fuse active triggering structure and a preparation process thereof. Background Art

[0002] A fuse is also called a current fuse. The IEC127 standard defines it as a fuse-link. It mainly serves as an overload protection. If the fuse is correctly placed in the circuit, the fuse will melt and cut off the current when the current abnormally rises to a certain height and temperature, thus protecting the safe operation of the circuit.

[0003] Existing fuses are generally classified into strip-shaped, sheet-shaped, glass tube-shaped, ceramic tube-shaped, plastic sheet-shaped with metal sheet-shaped pins, surface-mounted component type, and plug-in cylindrical type. However, these fuses are generally connected to the circuit in the form of thick film circuits. When an excessive current passes through the fuse, the fuse will be blown. However, generally, when there is a large current in the circuit, there will be more abnormal conditions in the entire electronic circuit. At this time, the fuse is passively blown, which can only reduce the generation and spread of losses, but cannot avoid the generation of losses.

[0004] In the lithium battery related industry, in order to reduce the fire and explosion caused by overcharging, over-discharging and short circuit failure of lithium-ion batteries, companies now produce three-terminal fuses to prevent and protect the above usage scenarios.

[0005] The existing three-terminal fuse generally includes three terminals, two of which are connected in series with the fuse piece, and the third terminal is used to heat the fuse piece. When overcharged, over-discharged or short-circuited, the third terminal generates a large amount of heat to actively heat and fuse the fuse piece.

[0006] Furthermore, after the existing fuse is triggered, the carrier carrying the fuse will break due to the high temperature, thereby causing damage to the circuit board. Summary of the invention

[0007] In view of the above situation, in order to overcome the defects of the prior art, the purpose of the present invention is to provide a fuse active triggering structure and a preparation process thereof, which effectively solves the problem that the existing fuse can only be blown passively and cannot detect abnormalities in advance and blow, thereby better protecting the entire circuit.

[0008] The technical solution solved by the present invention is a fuse active triggering structure, including a ceramic substrate, a resistor paste printed and burned in the ceramic substrate, a positive electrode arranged on one side of the ceramic substrate and connected to one end of the resistor paste, a negative electrode arranged on the other side of the ceramic substrate and connected to the other end of the resistor paste, and connecting contacts arranged on both sides of the positive electrode and the negative electrode, the ceramic substrate is divided into a positive plate and a negative plate in sequence along its thickness direction, the positive plate and the negative plate are bonded, and the resistor paste is printed and burned on the bonding surface of the positive plate and the negative plate.

[0009] Preferably, a positive electrode hole for use with one end of the resistor paste is provided on the bonding surface of the positive electrode plate printed with the resistor paste, and the resistor paste is filled in the positive electrode hole and communicated with the positive electrode.

[0010] Preferably, a negative electrode hole for use with the other end of the resistor paste is provided on the adhesive surface of the negative electrode plate printed with the resistor paste, and the resistor paste is filled in the negative electrode hole and communicated with the negative electrode.

[0011] Preferably, the resistor paste includes two contact portions for connecting the positive or negative electrode, and a heating portion disposed between the two contact portions, wherein an end of the heating portion is connected to the contact portion.

[0012] Preferably, the connection contacts include contact holes opened on the ceramic substrate and located on both sides of the resistor paste, and the contact holes are filled with electrode paste.

[0013] Preferably, the resistor paste composition consists of 50%-98% tungsten powder and 2%-50% porcelain powder, and the electrode paste composition consists of 90%-98% tungsten powder and 2%-10% porcelain powder.

[0014] A preparation process of a fuse active triggering structure comprises the following steps:

[0015] Step 1: sheet material preparation, selecting two alumina tape-cast green sheets with a double-layer shrinkage ratio of 1.15-1.18, respectively performing a punching process on the two alumina tape-cast green sheets to open positive electrode holes and negative electrode holes, and respectively performing a punching process on the two alumina tape-cast green sheets to open contact holes, to prepare positive and negative electrode plates;

[0016] Step 2: Preparation of the resistance wire plate. Under the conditions of temperature of 20-30℃ and humidity of 30%-70%, print the corresponding resistance paste circuit on the bonding surface of the positive plate or negative plate. After drying, the upper mold temperature is 65-75℃, the lower mold temperature is 75-85℃, and the pressure value is 80-120kg / cm 2 Under the following conditions, the positive electrode plate and the negative electrode plate are aligned, bonded, and hot pressed for 8-13 seconds to prepare a resistance wire plate body;

[0017] Step 3: External circuit printing: fill the contact holes on the resistance wire plate prepared in step 2 with slurry at a temperature of 20-30°C and a humidity of 30%-70%, and print the positive electrode or negative electrode on the corresponding end surface of the resistance wire plate to form a co-fired fuse blank;

[0018] Step 4: Firing, flattening and testing. A protective atmosphere is formed by humidifying hydrogen or nitrogen-hydrogen mixed gas, and the co-fired fuse blank is fired at a temperature of 1500-1650°C for 30-150 minutes to obtain a co-fired fuse ceramic substrate; after being placed at room temperature for a period of time, the co-fired fuse ceramic substrate is flattened and fired at a temperature of 1300-1500°C in the same atmosphere; it is placed at a temperature of 23-27°C and a humidity of 30%-70% for not less than 30 minutes to obtain a finished co-fired fuse ceramic substrate, and the prepared co-fired fuse ceramic substrate is tested for resistance using a milliohm pen.

[0019] Preferably, the double-layer high-temperature firing shrinkage ratio of the two alumina tape-cast green bodies in step 1 is 1.165±0.015.

[0020] Preferably, the bonding hot pressing in step 2 is divided into pressing down and holding pressure, the pressing down time is 3-30s, and the holding pressure time is 1-50s.

[0021] Preferably, in the step 4, the firing temperature of the co-fired fuse blank is 1500-1650°C, and the flattening firing temperature of the co-fired fuse ceramic substrate is 1300-1500°C.

[0022] The beneficial effects of the present invention are:

[0023] The resistor paste is printed and fired into the ceramic substrate using a co-fired structure. At the same time, a contact hole connected to the fuse is opened in the ceramic substrate. The fuse is connected through the contact hole and controlled by the resistor paste, so that the fuse can be blown before an abnormality occurs.

[0024] The resistance range between the positive and negative electrodes of the ceramic plate prepared by the present invention is less than 10 milliohms. Under this resistance, a large current can be generated instantaneously, and a large amount of heat can be generated in a short time, so that the fuse can be melted more quickly. After the monitoring device outside the present invention detects an abnormality, the present invention can respond more quickly to avoid causing additional losses. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a three-dimensional structural schematic diagram of the present invention;

[0026] Figure 2 It is a cutaway main view structural stereoscopic diagram of the present invention;

[0027] Figure 3 It is a cutaway right-side perspective structural schematic diagram of the present invention;

[0028] Figure 4 It is a schematic diagram of the main stereoscopic structure of the present invention after removing the positive electrode and the negative electrode;

[0029] Figure 5 It is a rear view stereoscopic structural schematic diagram of the present invention after the positive electrode and the negative electrode are removed;

[0030] In the figure, 1-ceramic substrate; 2-positive electrode; 3-negative electrode; 4-connection contact; 5-positive electrode hole; 6-negative electrode hole; 7-contact part; 8-heating wire; 9-contact hole; 10-electrode slurry. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by relevant technicians in the field without creative work are within the scope of protection of the present invention; Example

[0032] Step 1: sheet material preparation, selecting two alumina tape-cast green sheets with a double-layer shrinkage ratio of 1.15, and performing punching and punching processes on the two alumina tape-cast green sheets with the matte surface facing upward to prepare positive and negative plates, wherein the positive electrode hole opened by the punching process is located on the right side of the alumina tape-cast green sheet, and the negative electrode hole opened by the punching process is located on the left side of the alumina tape-cast green sheet;

[0033] Step 2: Preparation of the resistor wire plate. Print the resistor paste on the matte surface of the positive plate or negative plate prepared in step 1 at a temperature range of 22-28°C and a humidity range of 30%-70%. After printing, use a dryer to dry the plate. Lay the positive plate or negative plate printed with the resistor paste relatively close to each other. Use a flat hot press at an upper mold temperature of 70±1°C, a lower mold temperature of 80±1°C, and a mold pressure of 100kg / cm 2 The resistance wire plate was prepared by pressing down for 9±0.5 s and maintaining the pressure for 2±0.5 s under the condition;

[0034] Step 3: External circuit printing: fill the contact holes on the resistance wire plate prepared in step 2 with slurry under the conditions of a temperature range of 22-28°C and a humidity range of 30%-70%, print the positive electrode or negative electrode on the corresponding end surface of the resistance wire plate to form a co-fired fuse blank, and dry it in a dryer after printing;

[0035] Step 4: Firing and testing, firing the co-fired fuse blank at 1560°C to obtain a co-fired fuse ceramic substrate, placing it at room temperature for a period of time and then flattening it at 1470°C to prepare a finished co-fired fuse ceramic substrate, and using a milliohm pen to clamp the positive electrode and the negative electrode to perform a resistance test at room temperature, and the resistance range is measured to be 10-12 milliohms;

[0036] When in use, a fuse is welded between the two connection contacts, a power source is connected between the positive electrode and the negative electrode, and the power source and the resistor paste form a closed loop. When the power is turned on, the resistor paste instantly emits a large amount of heat, which melts the fuse welded between the two connection contacts, thereby disconnecting the circuit and protecting the circuit. The fuse produced under the conditions of this embodiment takes 4-5 seconds to melt the fuse. Example

[0037] Step 1: sheet material preparation, selecting two alumina tape-cast green sheets with a double-layer shrinkage ratio of 1.165, and performing punching and punching processes on the two alumina tape-cast green sheets with the matte surface facing upward to prepare positive and negative plates, wherein the positive electrode hole opened by the punching process is located on the right side of the alumina tape-cast green sheet, and the negative electrode hole opened by the punching process is located on the left side of the alumina tape-cast green sheet;

[0038] Step 2: Preparation of the resistor wire plate. Print the resistor paste on the matte surface of the positive plate or negative plate prepared in step 1 at a temperature range of 22-28°C and a humidity range of 30%-70%. After printing, use a dryer to dry the plate. Lay the positive plate or negative plate printed with the resistor paste relatively close to each other. Use a flat hot press at an upper mold temperature of 70°C, a lower mold temperature of 80°C, and a mold pressure of 100kg / cm 2 Under the condition, the pressure is pressed down for 9s and maintained for 2s to prepare the resistance wire plate;

[0039] Step 3: External circuit printing: fill the contact holes on the resistance wire plate prepared in step 2 with slurry under the conditions of a temperature range of 22-28°C and a humidity range of 30%-70%, print the positive electrode or negative electrode on the corresponding end surface of the resistance wire plate to form a co-fired fuse blank, and dry it in a dryer after printing;

[0040] Step 4: Firing and testing, firing the co-fired fuse blank at 1560°C to obtain a co-fired fuse ceramic substrate, placing it at room temperature for a period of time and then flattening it at 1470°C to prepare a finished co-fired fuse ceramic substrate, and using a milliohm pen to clamp the positive electrode and the negative electrode for resistance testing at a temperature of 23-27°C and a humidity of 30%-70%, the resistance range is 4-6 milliohms;

[0041] When in use, a fuse is welded between the two connection contacts, a power source is connected between the positive electrode and the negative electrode, and the power source and the resistor paste form a closed loop. When the power source is turned on, the resistor paste instantly emits a large amount of heat, which melts the fuse welded between the two connection contacts, thereby disconnecting the circuit and protecting the circuit. The fuse produced under the conditions of this embodiment takes 1-2 seconds to melt the fuse. Example

[0042] Step 1: sheet material preparation, selecting two alumina tape-cast green sheets with a double-layer shrinkage ratio of 1.165, and performing punching and punching processes on the two alumina tape-cast green sheets with the matte surface facing upward to prepare positive and negative plates, wherein the positive electrode hole opened by the punching process is located on the right side of the alumina tape-cast green sheet, and the negative electrode hole opened by the punching process is located on the left side of the alumina tape-cast green sheet;

[0043] Step 2: Preparation of the resistor wire plate. Print the resistor paste on the matte surface of the positive plate or negative plate prepared in step 1 at a temperature range of 22-28°C and a humidity range of 30%-70%. After printing, use a dryer to dry the plate. Lay the positive plate or negative plate printed with the resistor paste relatively close to each other. Use a flat hot press at an upper mold temperature of 70±1°C, a lower mold temperature of 80±1°C, and a mold pressure of 100kg / cm 2 Under the condition, press down for 9±1s and maintain the pressure for 2s to prepare the resistance wire plate;

[0044] Step 3: External circuit printing: fill the contact holes on the resistance wire plate prepared in step 2 with slurry under the conditions of a temperature range of 22-28°C and a humidity range of 30%-70%, print the positive electrode or negative electrode on the corresponding end surface of the resistance wire plate to form a co-fired fuse blank, and dry it in a dryer after printing;

[0045] Step 4: Firing and testing, firing the co-fired fuse blank at 1500°C to obtain a co-fired fuse ceramic substrate, placing it at room temperature for a period of time and then flattening it at 1470°C to prepare a finished co-fired fuse ceramic substrate, and using a milliohm pen to clamp the positive electrode and the negative electrode to perform a resistance test at room temperature, and the resistance range is 10-12 milliohms;

[0046] When in use, a fuse is welded between the two connection contacts, a power source is connected between the positive electrode and the negative electrode, and the power source and the resistor paste form a closed loop. When the power is turned on, the resistor paste instantly emits a large amount of heat, which melts the fuse welded between the two connection contacts, thereby disconnecting the circuit and protecting the circuit. The fuse produced under the conditions of this embodiment takes 4-5 seconds to melt the fuse. Example

[0047] Step 1: sheet material preparation, selecting two alumina tape-cast green sheets with a double-layer shrinkage ratio of 1.165, and performing punching and punching processes on the two alumina tape-cast green sheets with the matte surface facing upward to prepare positive and negative plates, wherein the positive electrode hole opened by the punching process is located on the right side of the alumina tape-cast green sheet, and the negative electrode hole opened by the punching process is located on the left side of the alumina tape-cast green sheet;

[0048] Step 2: Preparation of the resistor wire plate. Print the resistor paste on the matte surface of the positive plate or negative plate prepared in step 1 at a temperature range of 22-28°C and a humidity range of 30%-70%. After printing, use a dryer to dry the plate. Lay the positive plate or negative plate printed with the resistor paste relatively close to each other. Use a flat hot press at an upper mold temperature of 70±1°C, a lower mold temperature of 80±1°C, and a mold pressure of 100kg / cm 2 Under the condition, press down for 9±1s and maintain the pressure for 2s to prepare the resistance wire plate;

[0049] Step 3: External circuit printing: fill the contact holes on the resistance wire plate prepared in step 2 with slurry under the conditions of a temperature range of 22-28°C and a humidity range of 30%-70%, print the positive electrode or negative electrode on the corresponding end surface of the resistance wire plate to form a co-fired fuse blank, and dry it in a dryer after printing;

[0050] Step 4: Firing and testing, firing the co-fired fuse blank at 1600°C to obtain a co-fired fuse ceramic substrate, placing it at room temperature for a period of time and then flattening it at 1500°C to prepare a finished co-fired fuse ceramic substrate, and using a milliohm pen to clamp the positive electrode and the negative electrode to perform a resistance test at room temperature, and the resistance range is 7-9 milliohms;

[0051] When in use, a fuse is welded between the two connection contacts, a power source is connected between the positive electrode and the negative electrode, and the power source and the resistor paste form a closed loop. When the power is turned on, the resistor paste instantly emits a large amount of heat, which melts the fuse welded between the two connection contacts, thereby disconnecting the circuit and protecting the circuit. The fuse produced under the conditions of this embodiment takes 3-5 seconds to melt the fuse.

[0052] In summary, embodiment 2 is the optimal embodiment. The resistance range of the prepared co-fired fuse is less than 10 milliohms. At this resistance, a large current can be generated instantaneously, and a large amount of heat can be generated in a short time, so that the fuse can be melted more quickly. After the monitoring device outside the present invention detects an abnormality, the present invention can respond more quickly to avoid causing additional losses.

Claims

1. A fuse active trigger structure, comprising a ceramic substrate (1), wherein the ceramic substrate (1) is formed by high-temperature sintering of an alumina tape-cast green body, a resistor paste printed and fired into the ceramic substrate (1), a positive electrode (2) arranged on one side of the ceramic substrate (1) and connected to one end of the resistor paste, a negative electrode (3) arranged on the other side of the ceramic substrate (1) and connected to the other end of the resistor paste, and connection contacts (4) arranged on both sides of the positive electrode (2) and the negative electrode (3), characterized in that: The ceramic substrate (1) is divided into a positive electrode plate and a negative electrode plate in sequence along its thickness direction, the positive electrode plate and the negative electrode plate are bonded by hot pressing, and the resistor paste is printed and burned on the bonding surface of the positive electrode plate and the negative electrode plate; A positive electrode hole (5) used in conjunction with one end of the resistor paste is provided on the bonding surface of the positive electrode plate printed with the resistor paste, and the positive electrode hole (5) is filled with the electrode paste (10) and is connected to the positive electrode (2); A negative electrode hole (6) used in conjunction with the other end of the resistor paste is provided on the adhesive surface of the negative electrode plate printed with the resistor paste, and the negative electrode hole (6) is filled with electrode paste (10) and is connected to the negative electrode (3).

2. A fuse active triggering structure according to claim 1, characterized in that: The resistor paste comprises two contact portions (7) for connecting a positive or negative electrode (3), and a heating portion (8) arranged between the two contact portions (7), wherein an end of the heating portion (8) is connected to the contact portion (7).

3. A fuse active triggering structure according to claim 1, characterized in that: The connecting contact (4) comprises a contact hole (9) opened on the ceramic substrate (1) and located on both sides of the resistor paste, and the contact hole (9) is filled with electrode paste (10).

4. A fuse active triggering structure according to claim 3, characterized in that: The resistor paste composition consists of 50%-98% tungsten powder and 2%-50% porcelain powder, and the electrode paste (10) composition consists of 90%-98% tungsten powder and 2%-10% porcelain powder.

5. A process for preparing a fuse active triggering structure, used for preparing the fuse active triggering structure as claimed in claim 1, characterized in that: The following steps are involved: Step 1: sheet material preparation, selecting two alumina tape-cast green sheets with a double-layer shrinkage ratio of 1.15-1.18, respectively performing a punching process on the two alumina tape-cast green sheets to open positive electrode holes (5) and negative electrode holes (6), and respectively performing a punching process on the two alumina tape-cast green sheets to open contact holes (9), thereby preparing positive and negative electrode plates; Step 2: Preparation of the resistance wire plate. Under the conditions of temperature of 20-30℃ and humidity of 30%-70%, print the corresponding resistance paste circuit on the bonding surface of the positive plate or negative plate. After drying, the upper mold temperature is 65-75℃, the lower mold temperature is 75-85℃, and the pressure value is 80-120kg / cm 2 Under the following conditions, the positive electrode plate and the negative electrode plate are aligned, bonded, and hot pressed for 8-13 seconds to prepare a resistance wire plate body; Step 3: external circuit printing, under the conditions of a temperature of 20-30°C and a humidity of 30%-70%, the contact holes (9) on the resistance wire plate prepared in step 2 are filled with slurry, and at the same time, a positive electrode (2) or a negative electrode (3) is printed on the corresponding end surface of the resistance wire plate to form a co-fired fuse blank; Step 4: Firing, leveling and testing. A protective atmosphere is formed by humidifying hydrogen or nitrogen-hydrogen mixed gas, and the co-fired fuse blank is fired at a temperature of 1500-1650°C for 30-150 minutes to obtain a co-fired fuse ceramic substrate; after being placed at room temperature for a period of time, the co-fired fuse ceramic substrate is leveled and fired at a temperature of 1300-1500°C in the same atmosphere; after leveling, it is placed at a temperature of 23-27°C and a humidity of 30%-70% for not less than 30 minutes to obtain a finished co-fired fuse ceramic substrate, and the prepared co-fired fuse ceramic substrate is tested for resistance using a milliohm pen.

6. The preparation process of a fuse active trigger structure according to claim 5, characterized in that: In the step 2, the bonding hot pressing is divided into pressing down and holding pressure, the pressing down time is 3-30s, and the holding pressure time is 1-50s.

Citation Information

Patent Citations

  • Thin type self-control protector and manufacturing method thereof

    CN105576598A

  • Ceramic chip fuse having internal heating member

    KR101307530B1