Geopolymer composition, geopolymer and preparation method and application thereof
By using specific proportions of water glass, magnesium-containing components, hydrated gypsum and carbon fibers in geopolymers to optimize the hydration reaction, the problems of long setting time and low compressive strength of geopolymer materials are solved, achieving faster Condensation and higher early compressive strength, suitable for emergency repair projects.
Patent Information
- Application Number
- CN202410837314.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-26
AI Technical Summary
The setting time of existing geopolymer materials is too long to meet the needs of emergency repair projects. At the same time, its compressive strength is insufficient to meet the actual requirements of engineering construction.
A geopolymer composition is used, including basic components, water glass, magnesium-containing components, hydrated gypsum and carbon fiber. Through the synergy of specific proportions of components, the hydration reaction is optimized, the setting speed and early strength are improved, and the The material has high compressive strength in the early stages of construction.
It achieves a more suitable setting time and fluidity of the geopolymer, avoids shrinkage cracks caused by too rapid setting, and provides extremely high early compressive strength, which is particularly suitable for use in the field of road engineering repair.
Smart Images

Figure CN118405865B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of cement materials, and in particular to a geopolymer composition, a geopolymer, and a preparation method and application thereof. Background Art
[0002] Ordinary Portland cement suffers from various degrees of damage, cracking, etc. due to natural disasters and external forces during its long-term use in civil engineering.
[0003] For daily maintenance and emergency repair of industrial and civil roads such as highways, airport pavements, municipal trunk roads, seaports, docks, etc., rapid repair is crucial to ensure smooth traffic and normal production; therefore, engineering emergency repair materials that can solidify super quickly are needed.
[0004] However, while achieving ultra-fast solidification, it is also necessary to ensure that the engineering repair materials have good compressive strength after solidification to meet the actual engineering construction requirements.
[0005] Geopolymer is an inorganic polymer material formed by chemically stimulating bulk solid waste as the main raw material. Compared with ordinary Portland cement, the production of geopolymer does not require the mining of limestone, which greatly reduces CO2 emissions.
[0006] In addition, geopolymers have the advantages of fast setting speed, strong acid and alkali resistance, excellent weather resistance, and good flame retardancy. Therefore, they have received more and more attention.
[0007] CN115557739A discloses a marine geopolymer material, comprising the following weight components: 25-60 parts of slag powder, 10-30 parts of ground basalt powder, 5-25 parts of metakaolin, 5-20 parts of light-burned magnesium powder, 2.5-15 parts of anhydrite, 0.1-25 parts of sea sand, 2.5-5 parts of fly ash microbeads, 0.1-1.5 parts of basalt chopped fibers, 0.1-2 parts of microfibers, 5-30 parts of water glass, 3-15 parts of alkaline activator, 0.1-3 parts of composite rust inhibitor, and 0.4-1 parts of water reducer. However, the coagulation time of the geopolymer material in the prior art is relatively long, and it cannot meet the needs of emergency repair projects. Summary of the invention
[0008] The purpose of the invention is to overcome the problems of long setting time of cement materials and low compressive strength after construction in the prior art.
[0009] In order to achieve the above object, the first aspect of the present invention provides a geopolymer composition, which comprises: a base component, water glass, a magnesium-containing component, hydrated gypsum and carbon fiber;
[0010] Relative to 100 parts by weight of the base component, the content of the water glass is 55-65 parts by weight, the content of the magnesium-containing component is 5-6 parts by weight, the content of the hydrated gypsum is 1-3 parts by weight, and the content of the carbon fiber is 2-3 parts by weight;
[0011] Based on the total weight of the basic component, the basic component contains 80-95wt% of metallurgical slag powder and 5-20wt% of metakaolin; the specific surface area of the metallurgical slag powder is 550-750m 2 / kg;
[0012] The modulus of the water glass is not less than 1.0;
[0013] The magnesium-containing component is a combination of magnesium oxide, magnesium carbonate and magnesium hydroxide in a mass ratio of 1:0.1-0.3:0.2-0.5;
[0014] The hydrated gypsum is a combination of hemihydrate gypsum and anhydrous gypsum in a mass ratio of 1:1-3.
[0015] The second aspect of the present invention provides a method for preparing a geopolymer, which is carried out using the components in the geopolymer composition described in the first aspect, comprising:
[0016] The geopolymer slurry containing the components of the geopolymer composition is subjected to curing treatment to obtain the geopolymer.
[0017] The third aspect of the present invention provides a geopolymer prepared by the method described in the second aspect.
[0018] The fourth aspect of the present invention provides the use of the geopolymer described in the third aspect in emergency repair engineering.
[0019] The raw materials in the geopolymer composition provided by the invention have a wide range of sources, and do not require the mining of limestone, so the composition is environmentally friendly.
[0020] The components with specific contents in the geopolymer composition provided by the present invention cooperate with each other, so that the prepared geopolymer has more suitable setting time, better fluidity and stability.
[0021] The geopolymer provided by the present invention is easy to construct and cast, has extremely high compressive strength in the early stage of construction, and will not produce shrinkage cracks caused by too fast coagulation, and is particularly suitable for application in the field of road engineering repair.
[0022] After research, the inventor believes that the mechanism involved in the present invention mainly includes:
[0023] (1) The three magnesium-containing compounds in the magnesium-containing component (a combination of magnesium oxide, magnesium carbonate and magnesium hydroxide in a mass ratio of 1:0.1-0.3:0.2-0.5) of the present invention interact with each other when combined in a specific ratio, and act together on the hydration process of the alkali-activated cementitious material. Among them, magnesium oxide and magnesium hydroxide can quickly increase the pH value of the reaction system, while magnesium carbonate may regulate this process to a certain extent to avoid the adverse effects caused by excessively high pH values. The specific combination of these three magnesium-containing compounds can optimize the composition and microstructure of the hydration product, making the geopolymer structure more compact, thereby improving the setting speed and early strength of the geopolymer.
[0024] Specifically, magnesium oxide releases heat during the hydration process, which increases the temperature of the composition and accelerates the hydration reaction. When magnesium oxide absorbs water, it generates magnesium hydroxide, which can increase the pH value of the reaction system and provide more favorable conditions for the dissolution and polymerization of silicate minerals in the composition. At the same time, the hydration product of magnesium oxide interacts with hydrated calcium aluminosilicate gel (C-(A)-SH gel) to form a more stable gel structure. When magnesium carbonate comes into contact with water, it generates magnesium bicarbonate and hydroxide ions, which help maintain the alkaline environment of the solution. In addition, the hydrolysis of magnesium carbonate may produce some Mg 2+ These ions can participate in the hydration reaction and promote the coagulation of the cementitious material. 2+ and OH - It can directly participate in the hydration reaction to accelerate the setting process; and the products formed by the participation of magnesium hydroxide in the reaction, such as hydrotalcite and MSH, help to improve the early strength of geopolymers.
[0025] (2) The specific hydrated gypsum of the present invention (a combination of hemihydrate gypsum and anhydrous gypsum in a mass ratio of 1:1-3) can jointly adjust the fluidity and setting time of the geopolymer.
[0026] Specifically, hemihydrate gypsum absorbs some free water during the hydration process to form dihydrate gypsum (CaSO4·2H2O), which consumes some water and affects the setting time of geopolymers. The dihydrate gypsum formed during the hydration of hemihydrate gypsum has a lower density and better dispersibility, and the hydration product of dihydrate gypsum can form a network structure, which helps to maintain the fluidity of the material. Anhydrous gypsum needs to absorb water during the hydration process to form hemihydrate gypsum or dihydrate gypsum. At the same time, the hydration product of anhydrous gypsum can form a skeleton structure, which helps to improve the fluidity and plasticity of geopolymers. When hemihydrate gypsum and anhydrous gypsum are combined in a specific ratio (the mass ratio of hemihydrate gypsum to anhydrous gypsum is 1:1-3), they can complement each other and cooperate with each other, so that the obtained geopolymer has better fluidity and more suitable setting time. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 is the in-situ Raman average spectrum of the geopolymer slurry obtained in step (1) of Example 1 of the present invention at 0-60 min and the contour Raman;
[0028] Figure 2 This is the Raman imaging image of the geopolymer slurry obtained in step (1) of Example 1 of the present invention at the 60th minute of the analysis time. DETAILED DESCRIPTION
[0029] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0030] As mentioned above, the first aspect of the present invention provides a composition for geopolymers, the composition comprising: a base component, water glass, a magnesium-containing component, hydrated gypsum and carbon fibers;
[0031] Relative to 100 parts by weight of the base component, the content of the water glass is 55-65 parts by weight, the content of the magnesium-containing component is 5-6 parts by weight, the content of the hydrated gypsum is 1-3 parts by weight, and the content of the carbon fiber is 2-3 parts by weight;
[0032] Based on the total weight of the basic component, the basic component contains 80-95wt% of metallurgical slag powder and 5-20wt% of metakaolin; the specific surface area of the metallurgical slag powder is 550-750m 2 / kg;
[0033] The modulus of the water glass is not less than 1.0;
[0034] The magnesium-containing component is a combination of magnesium oxide, magnesium carbonate and magnesium hydroxide in a mass ratio of 1:0.1-0.3:0.2-0.5;
[0035] The hydrated gypsum is a combination of hemihydrate gypsum and anhydrous gypsum in a mass ratio of 1:1-3.
[0036] Preferably, the hydrated gypsum is a combination of hemihydrate gypsum and anhydrous gypsum in a mass ratio of 1:1-1.5. The inventors of the present invention have found that in this preferred case, the obtained geopolymer has a more suitable setting time and will not produce shrinkage cracks caused by too fast setting.
[0037] Preferably, the average particle diameter of the hydrated gypsum is 0.1-10 μm.
[0038] Preferably, the average length of the carbon fibers is 1-4 mm, and the elastic modulus is 200-300 GPa. The inventors of the present invention have found that in this preferred case, the obtained geopolymer has a more suitable setting time.
[0039] Preferably, the average particle diameter of the magnesium-containing component is 0.1-10 μm.
[0040] Preferably, the water glass is sodium water glass and / or potassium water glass, and the modulus of the water glass is 1.0-1.5, and the solid content is 40wt%-50wt%. The inventors of the present invention have found that in this preferred case, the obtained geopolymer has better fluidity and higher early strength.
[0041] Preferably, the water glass is sodium water glass.
[0042] Preferably, the metallurgical slag powder contains 25-40wt% silicon dioxide, 15-25wt% aluminum oxide and 30-40wt% calcium oxide.
[0043] According to a preferred embodiment, the metakaolin is a product obtained by calcining kaolin and / or kaolinite;
[0044] The calcination treatment is carried out at a temperature of 800-1000° C. and for a time of 2-8 hours.
[0045] Preferably, the metakaolin is a product obtained by sequentially grinding and calcining kaolin and / or kaolinite.
[0046] The present invention has no special requirements for the grinding method, and those skilled in the art can select it according to their needs.
[0047] Preferably, the content of silicon dioxide in the kaolin and the kaolinite is independently 45-65wt%, and the content of aluminum oxide is independently 35-55wt%.
[0048] As mentioned above, the second aspect of the present invention provides a method for preparing a geopolymer, which is carried out using the components in the geopolymer composition described in the first aspect, comprising:
[0049] The geopolymer slurry containing the components of the geopolymer composition is subjected to curing treatment to obtain the geopolymer.
[0050] Preferably, before the curing treatment, the process further comprises stirring the components in the geopolymer composition to obtain a geopolymer slurry.
[0051] Preferably, the stirring treatment conditions include: temperature of 10-30° C., rotation speed of 100-150 rpm, and time of 2-5 min.
[0052] Preferably, the curing treatment conditions include: temperature of 20-40°C and humidity of 90-100%.
[0053] As mentioned above, the third aspect of the present invention provides a geopolymer prepared by the method described in the second aspect.
[0054] As mentioned above, the fourth aspect of the present invention provides the use of the geopolymer described in the third aspect in emergency repair engineering.
[0055] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the instruments, reagents, materials, etc. involved are all conventional instruments, reagents, materials, etc., which can be obtained through regular commercial channels. Among them, unless otherwise specified, the reagents used are all commercially available analytically pure products.
[0056] Metallurgical slag powder :
[0057] Metallurgical slag powder I:
[0058] The content of silicon dioxide is 30-32wt%, the content of aluminum oxide is 16-18wt%, the content of calcium oxide is 34-36wt%, and the specific surface area is 700m 2 / kg, purchased from Hunan Ningying New Material Technology Co., Ltd.
[0059] Metallurgical slag powder II: The content of silicon dioxide is 32-33wt%, the content of aluminum oxide is 16-18wt%, the content of calcium oxide is 38-40wt%, and the specific surface area is 450m 2 / kg, purchased from Jiyuan Guotai Industrial Co., Ltd.
[0060] Magnesium-containing ingredients:
[0061] The magnesium-containing component I includes magnesium oxide, magnesium carbonate and magnesium hydroxide in a mass ratio of 1:0.1:0.3, and the average particle diameter is 1 μm.
[0062] Magnesium-containing component II: magnesium oxide, magnesium carbonate and magnesium hydroxide in a mass ratio of 1:0.5:0.3, with an average particle diameter of 1 μm.
[0063] Kaolin: The content of silicon dioxide is 54.6wt%, and the content of aluminum oxide is 39.3wt%, which is purchased from Lingshou County Yixin Mineral Products Co., Ltd.
[0064] Kaolinite: The content of silicon dioxide is 46.5wt%, and the content of aluminum oxide is 39.5wt%, which was purchased from Lingshou County Yixin Mineral Products Co., Ltd.
[0065] Water Glass:
[0066] Sodium water glass: The modulus number is 3.3, purchased from Jiashan Yourui Refractory Material Co., Ltd., brand number is SP38.
[0067] Sodium water glass I, modulus 1.2, solid content 42.5wt%, homemade (prepared according to the mass ratio of sodium hydroxide to sodium water glass of 1:5.27).
[0068] Sodium water glass II, modulus of 0.5, solid content of 51.3wt%, homemade (prepared according to the mass ratio of sodium hydroxide to sodium water glass: 1:1.62).
[0069] Carbon Fiber:
[0070] Carbon fiber I: average length is 3 mm, elastic modulus is 200 GPa, purchased from Dongguan Wanlixiang Carbon Fiber Co., Ltd., customized.
[0071] Carbon fiber II: average length is 5 mm, elastic modulus is 150 GPa, purchased from Dongguan Wanlixiang Carbon Fiber Co., Ltd., customized.
[0072] Hydrated gypsum:
[0073] Hydrated gypsum I: A combination of hemihydrate gypsum and anhydrous gypsum in a mass ratio of 1:1, with an average particle diameter of 4 μm.
[0074] Hydrate II: A combination of hemihydrate gypsum and anhydrous gypsum in a mass ratio of 1:3, with an average particle diameter of 4 μm.
[0075] Hydrated gypsum III: A combination of hemihydrate gypsum and anhydrous gypsum in a mass ratio of 1:4, with an average particle diameter of 4 μm.
[0076] Hemihydrate gypsum: purchased from Henan Juneng New Building Materials Co., Ltd.
[0077] Anhydrous gypsum: purchased from Henan Juneng New Building Materials Co., Ltd.
[0078] Different raw material formulations are used in the following examples of the present invention. Unless otherwise specified, all raw material amounts are parts by weight, and each part by weight represents 6 g.
[0079] Preparation Example 1
[0080] 1200 g of kaolin and 800 g of kaolinite were sequentially ground and calcined (temperature: 800° C., time: 4 h) to obtain metakaolin.
[0081] The average particle diameter of the metakaolin was tested by a laser particle size analyzer, and the average particle diameter of the metakaolin was found to be 8.28 μm.
[0082] Example 1
[0083] This example is used to illustrate that the geopolymer composition of the present invention is prepared according to the formulation of Table 1 and the following method.
[0084] The method for preparing the geopolymer comprises the following steps:
[0085] (1) stirring the base component, water glass, magnesium-containing component, hydrated gypsum I and carbon fiber to obtain a geopolymer slurry;
[0086] The stirring temperature was 20°C, the speed was 100 rpm, and the time was 3 min;
[0087] (2) Curing the geopolymer slurry to obtain the geopolymer.
[0088] Examples 2 to 6 are all carried out using a method similar to that of Example 1, except that the formulation dosage and process parameters are different, see Table 1 for details.
[0089] Example 7
[0090] This example is carried out in a similar manner to that of Example 1, except that an equal amount of hydrated gypsum II is used in this example to replace the hydrated gypsum I in Example 1, and the rest is the same as that of Example 1.
[0091] Example 8
[0092] This embodiment is carried out using a method similar to that of Embodiment 1, except that an equal weight portion of carbon fiber II is used to replace the carbon fiber I in Embodiment 1, and the rest is the same as that of Embodiment 1.
[0093] Comparative Example 1
[0094] This comparative example is carried out in a similar manner to Example 1, except that an equal weight portion of metallurgical slag powder II is used to replace the metallurgical slag powder I in Example 1, and the rest is the same as Example 1.
[0095] Comparative Example 2
[0096] This comparative example was carried out in a similar manner to Example 1, except that the amount of hydrated gypsum I in this comparative example was adjusted from 1 part by weight in Example 1 to 5 parts by weight, and the rest was the same as Example 1.
[0097] Comparative Example 3
[0098] This comparative example was carried out in a similar manner to Example 1, except that, while the amounts of the basic components were kept constant, the amount of metallurgical slag powder I in this comparative example was 70 parts by weight, the amount of metakaolin was 30 parts by weight, and the rest was the same as in Example 1.
[0099] Comparative Example 4
[0100] This comparative example was carried out in a similar manner to Example 1, except that the amount of sodium water glass I in this comparative example was adjusted from 60 parts by weight in Example 1 to 70 parts by weight, and the rest was the same as Example 1.
[0101] Comparative Example 5
[0102] This comparative example is carried out in a similar manner to Example 1, except that an equal weight portion of magnesium-containing component II is used to replace the magnesium-containing component I in Example 1, and the rest is the same as Example 1.
[0103] Comparative Example 6
[0104] This comparative example is carried out in a similar manner to Example 1, except that an equal amount of hemihydrate gypsum is used to replace the hydrated gypsum I in Example 1, and the rest is the same as Example 1.
[0105] Comparative Example 7
[0106] This comparative example is carried out in a similar manner to Example 1, except that anhydrous gypsum I in Example 1 is replaced with an equal weight portion of anhydrous gypsum in this comparative example, and the rest is the same as Example 1.
[0107] Comparative Example 8
[0108] This comparative example is carried out in a similar manner to Example 1, except that an equal amount of hydrated gypsum III is used to replace the hydrated gypsum I in Example 1, and the rest is the same as Example 1.
[0109] Comparative Example 9
[0110] This embodiment is carried out in a similar manner to that of Embodiment 1, except that an equal weight portion of sodium water glass II is used in this embodiment to replace the sodium water glass I in Embodiment 1, and the rest is the same as that of Embodiment 1.
[0111] Table 1
[0112]
[0113] Test Case
[0114] 1. The fluidity of the geopolymer prepared in the above example was tested by the method specified in GB / T 8077-2000; the setting time (including initial setting time and final setting time) of the geopolymer prepared in the above example was tested by the method specified in GB / T 1346-2011; the compressive strength of the geopolymer prepared in the above example was tested by the method specified in GB / T 17671-2021; the results of the above performance tests are shown in Table 2.
[0115] Table 2
[0116]
[0117] 2. The Raman spectrum information of the geopolymer slurry obtained in step (1) of Example 1 was analyzed using a confocal Raman spectrometer (analysis time 0-60 min). The results are as follows: Figure 1 (Contour map of the average in-situ Raman spectra at different analysis times) and Figure 2 (Raman imaging at 60 minutes of analysis time)
[0118] pass Figure 1 It can be seen that as the analysis time increases, the fingerprint peak of magnesia chalcite (wave number at 1400cm -1 ) peak intensity weakens, indicating that the components in the geopolymer slurry gradually react.
[0119] pass Figure 2 It can be seen that the distribution of hydrotalcite-like and calcium aluminosilicate hydrate gel (C-(A)-SH gel) rapidly generated by the geopolymer slurry obtained in step (1) of Example 1 of the present invention within 60 minutes can provide a more suitable setting time and higher early strength compared with calcium silicate hydrate (CSH), a cement hydration product.
[0120] It can be seen from the above results that the geopolymer prepared by the geopolymer composition provided by the present invention has better fluidity (fluidity is not less than 183mm) and more suitable setting time (initial setting time is 15-22min, final setting time is less than 30min. If the initial setting time is too short, it is not suitable for engineering practice); and the geopolymer provided by the present invention has extremely high compressive strength in the early stage of construction, and is particularly suitable for application in the field of emergency engineering repair.
[0121] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A geopolymer composition, characterized in that: The composition comprises: a basic component, water glass, a magnesium-containing component, hydrated gypsum and carbon fiber; Relative to 100 parts by weight of the base component, the content of the water glass is 55-65 parts by weight, the content of the magnesium-containing component is 5-6 parts by weight, the content of the hydrated gypsum is 1-3 parts by weight, and the content of the carbon fiber is 2-3 parts by weight; Based on the total weight of the basic component, the basic component contains 80-95wt% of metallurgical slag powder and 5-20wt% of metakaolin; the specific surface area of the metallurgical slag powder is 550-750m 2 / kg; The modulus of the water glass is not less than 1.0; The magnesium-containing component is a combination of magnesium oxide, magnesium carbonate and magnesium hydroxide in a mass ratio of 1:0.1-0.3:0.2-0.5; The hydrated gypsum is a combination of hemihydrate gypsum and anhydrous gypsum in a mass ratio of 1:1-3.
2. The composition according to claim 1, wherein The hydrated gypsum is a combination of hemihydrate gypsum and anhydrous gypsum in a mass ratio of 1:1-1.
5.
3. The composition according to claim 1 or 2, wherein The average length of the carbon fiber is 1-4 mm, and the elastic modulus is 200-300 GPa; And / or, the average particle diameter of the magnesium-containing component is 0.1-10 μm.
4. The composition according to claim 1 or 2, wherein The water glass is sodium water glass and / or potassium water glass, and the modulus of the water glass is 1.0-1.5, and the solid content is 40wt%-50wt%.
5. The composition according to claim 1 or 2, wherein The metallurgical slag powder has a silicon dioxide content of 25-40wt%, an aluminum oxide content of 15-25wt%, and a calcium oxide content of 30-40wt%.
6. The composition according to claim 1 or 2, wherein The metakaolin is a product obtained by calcining kaolin and / or kaolinite; The calcination treatment is carried out at a temperature of 800-1000° C. and for a time of 2-8 hours.
7. A method for preparing a geopolymer, characterized in that: The method is carried out using the components in the geopolymer composition according to any one of claims 1 to 6, comprising: The geopolymer slurry containing the components of the geopolymer composition is subjected to curing treatment to obtain the geopolymer.
8. The method according to claim 7, wherein: The curing conditions include: temperature of 20-40°C and humidity of 90-100%.
9. Geopolymer prepared by the method of claim 7 or 8.
10. Use of the geopolymer according to claim 9 in emergency repair projects.
Citation Information
Patent Citations
Phosphorus oxide magnesium gel material for 3D printing house
CN106396603A
Method for reinforcing lignin fiber soil stabilizer roadbed
CN107686323A