Acrylic foam tape and preparation method thereof
By introducing heat-resistant monomers to prepare modified polyacrylate, the problem of decreasing cohesion strength of acrylate pressure-sensitive adhesive in high-temperature environments is solved, and the heat resistance and impact resistance of acrylic foam tape are improved. Adapt to harsher application environments.
Patent Information
- Application Number
- CN202410474096.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-04-19
AI Technical Summary
The existing acrylate pressure-sensitive adhesives have a decrease in cohesion strength in high-temperature environments, and there are more residual adhesives during peeling, which limits their application in high-temperature environments such as high-temperature resistance and electronic components fixation.
The heat-resistant monomer is introduced to prepare modified polyacrylates, which improves thermal stability and cross-linking density through heterocyclic rings and aromatic rings, and enhances the heat resistance and stability of the polymer.
It significantly improves the heat resistance and impact resistance of acrylic foam tape, making it adapt to a harsh application environment, and reduces the residual glue problem during peeling.
Smart Images

Figure BDA0004799890270000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer compound compositions, and in particular to an acrylic foam tape and a preparation method thereof. Background Art
[0002] In order to meet consumers' dual demands for portability and aesthetics, modern consumer electronic products tend to be designed to be thinner and lighter, while achieving higher integration in terms of function. This trend means that more components need to be accommodated in a limited space, so the pressure-sensitive tape as an auxiliary fixing material must have sufficient space utilization, that is, the thickness must be reduced as much as possible while ensuring its function. In practical applications, the net thickness of most pressure-sensitive tape products is controlled within the range of 0.80 to 0.03 mm. In particular, those tapes with a thickness of more than 0.30 mm are usually used for structural bonding inside the product, such as fixing key parts such as the casing and frame. Users expect the tape to have sufficient thickness to achieve a good bonding effect while also being able to withstand the internal stress caused by dimensional tolerance matching or thermodynamic deformation to ensure the stability and reliability of the bonding. In this thickness range, double-sided tapes with foam as the substrate have become the leading product on the market due to their excellent energy absorption capacity and stress dispersion characteristics.
[0003] CN201610816218.3 provides an acrylic foam tape composition and a method for preparing the acrylic foam tape, comprising a foam substrate layer and tape layers on the upper and lower sides of the foam substrate layer; the foam substrate layer comprises the following components in parts by weight: 100 parts of acrylic mixture; 0.1 to 5 parts of reaction aid; 0.01 to 5 parts of bridging agent; 0.1 to 10 parts of porous filler; 1 to 10 parts of additives; the tape layer comprises the following components in parts by weight: 100 parts of acrylic mixture; 0.1 to 5 parts of reaction aid; 0.01 to 5 parts of bridging agent; 0.1 to 10 parts of tackifier; 1 to 10 parts of additives. The acrylic foam tape is used for pasting injection moldings of automobiles or electronic products, so that the injection moldings can be permanently and fixedly adhered to the body of the automobile and the electronic products, and has the function of preventing collisions between injection moldings and preventing noise.
[0004] CN202010201651.2 provides an anti-fouling acrylic foam tape and a preparation method thereof, comprising a foam substrate layer and a tape layer coated on the upper and lower sides of the foam substrate layer; the tape layer comprises the following components in parts by weight: 100 parts of acrylic mixture; 0.1 to 5 parts of photoreaction aid; 0.1 to 2 parts of thermal reaction aid; 0.01 to 5 parts of bridging agent; 2 to 10 parts of fluorine-containing polyurethane. The acrylic foam tape is used for pasting automobile exterior decorations, so that the exterior decorations can be permanently and fixedly adhered to the body of the car, and has self-cleaning and anti-fouling capabilities.
[0005] Acrylic foam plays an important role in the field of electronic display modules due to its excellent cushioning, protection, sealing and gap filling properties. Especially in the application of high-end display technologies such as flexible OLED screens and AMOLED, acrylic foam can effectively prevent screen breakage caused by external impact during manufacturing, transportation, installation and daily use. With the rapid development of the electronics industry, the display modules of equipment tend to be thinner and more portable, which poses a higher challenge to the high temperature resistance and impact resistance of acrylic foam materials. In order to ensure the long-term stability of display modules under various extreme environments, such as high temperature and high humidity conditions, manufacturers need to conduct rigorous testing and verification of these materials. Therefore, the improvement of these properties of acrylic foam is crucial to meeting the high standards of durability and reliability of modern electronic products. Summary of the invention
[0006] In view of the above-mentioned defects in the prior art, the technical problem to be solved by the present invention is to provide an acrylic foam tape and a preparation method thereof.
[0007] Ordinary acrylic pressure-sensitive adhesives will experience a sharp drop in modulus and cohesive strength in a high-temperature environment, becoming a nearly viscous body. When peeled off, a large amount of residual glue will appear on the surface of the adherend, which greatly limits its application in high-temperature environments such as high-temperature resistant shielding, electronic component tape fixation, and electronic component bonding. The main chain of acrylic ester is a saturated carbon-carbon structure with certain heat resistance. However, due to the low cross-linking density after polymerization, the molecular chain is prone to relative movement in a high-temperature environment, and the cohesive strength and bonding performance are significantly reduced. After peeling, the failure morphology is mainly cohesive failure, and there is a lot of residual glue. The present invention prepares modified polyacrylate by introducing heat-resistant monomers. Since heterocyclic rings and aromatic rings have good thermal stability, the heat resistance of the final product can be greatly improved, and the introduction of heat-resistant monomers also increases the cross-linking density at the same time, and the rigid structure of aromatic heterocyclic rings can also improve the stability of the polymer. Therefore, the acrylic foam tape finally obtained has strong impact resistance and high heat resistance, and can adapt to more severe application environments.
[0008] To achieve the above object, the present invention provides a method for preparing an acrylic foam tape, comprising the following steps:
[0009] The modified polyacrylate masterbatch, foamed microspheres, curing agent, dispersant, tackifier, filler and solvent are mixed and coated on the release film, and then heated and dried to remove the solvent.
[0010] The preparation method of the modified polyacrylate masterbatch comprises the following steps:
[0011] The product is prepared by mixing n-butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, 2-vinyl-4,6-diphenyl-1,3,5-triazine and benzoyl peroxide with ethyl acetate and heating and polymerizing the mixture for 2 to 3 hours under a nitrogen atmosphere.
[0012] Furthermore, the mass ratio of the modified polyacrylate masterbatch, foamed microspheres, curing agent, dispersant, tackifier, filler and solvent is 50-80:1-3:0.5-2:0.1-1:1-5:2-5:10-50.
[0013] Furthermore, the foamed microspheres are hollow glass microspheres.
[0014] Furthermore, the curing agent is one of an isocyanate curing agent, an epoxy curing agent, and a pyridine curing agent.
[0015] Furthermore, the dispersant is one of a condensate of fatty alcohol and ethylene oxide, sodium polyacrylate, and a nonionic polymer block copolymer.
[0016] Furthermore, the tackifier is a rosin-based resin.
[0017] Furthermore, the filler is carbon black.
[0018] Furthermore, the solvent is one of dimethyl carbonate, ethyl acetate and toluene.
[0019] Furthermore, the coating thickness is 50 to 150 μm.
[0020] Preferably, the method for preparing the modified polyacrylate masterbatch comprises the following steps:
[0021] n-Butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, 2-vinyl-4,6-diphenyl-1,3,5-triazine and benzoyl peroxide are mixed with ethyl acetate in a mass ratio of 80-100:2-5:5-10:2-8:0.1-0.5:100-200, and the mixture is heated to 65-80° C. in a nitrogen atmosphere and polymerized for 2-3 hours to obtain the product.
[0022] The invention also provides an acrylic foam tape, which is prepared by the above method.
[0023] Beneficial effects of the present invention:
[0024] Compared with the prior art, the present invention prepares modified polyacrylate by introducing heat-resistant monomers. Since heterocyclic rings and aromatic rings have good thermal stability, the heat resistance of the final product can be greatly improved. The introduction of heat-resistant monomers also increases the crosslinking density, and the rigid structure of aromatic heterocyclic rings can also improve the stability of the polymer. Therefore, the acrylic foam tape finally obtained has strong impact resistance and high heat resistance and can adapt to more severe application environments. DETAILED DESCRIPTION
[0025] Rosin-based resin, brand: Hercolyn D, produced by Hongji Plastics, Zhangmutou, Dongguan.
[0026] Hollow glass microspheres, particle size: 15-75 μm, model: VS5500, 3M.
[0027] Isocyanate curing agent, BASF HI100, Maoming Gaojun Petrochemical.
[0028] Non-ionic polymer block copolymer, model: DISUPER S9100, Guangdong Core New Materials.
[0029] Carbon black, particle size: 24 nm, model: MA-100, Mitsubishi, Japan.
[0030] PET release film, item number: S25TA3, Shenzhen Shunhexing Electronic Materials.
[0031] 2-ethenyl-4,6-diphenyl-1,3,5-triazine, CAS No.: 81854-87-7.
[0032] 2-ethenyl-4,6-dimethyl-1,3,5-triazine, CAS No.: 89853-50-9.
[0033] 4-ethenyl-6-phenyl-1,3,5-triazin-2-amine, CAS No.: 18120-43-9.
[0034] 1-phenyl-2-propenylbenzene, CAS No.: 3542-14-1.
[0035] Comparative Example 1
[0036] A method for preparing an acrylic foam tape comprises the following steps:
[0037] Polyacrylate masterbatch, hollow glass microspheres, isocyanate curing agent, nonionic polymer block copolymer, rosin-based resin, carbon black and ethyl acetate are mixed in a mass ratio of 65:2.5:0.8:0.5:2:3:45 and coated on a PET release film with a coating thickness of 100 μm. The mixture is heated and dried to remove the solvent.
[0038] The preparation method of the polyacrylate masterbatch comprises the following steps:
[0039] n-Butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, benzoyl peroxide and ethyl acetate are mixed in a mass ratio of 90:5:8:0.5:150, and the mixture is heated to 70° C. in a nitrogen atmosphere and polymerized for 3 hours to obtain the product.
[0040] Example 1
[0041] A method for preparing an acrylic foam tape comprises the following steps:
[0042] The modified polyacrylate masterbatch, hollow glass microspheres, isocyanate curing agent, nonionic polymer block copolymer, rosin-based resin, carbon black and ethyl acetate are mixed in a mass ratio of 65:2.5:0.8:0.5:2:3:45 and coated on a PET release film with a coating thickness of 100 μm. The mixture is heated and dried to remove the solvent.
[0043] The preparation method of the modified polyacrylate masterbatch comprises the following steps:
[0044] n-Butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, 2-vinyl-4,6-diphenyl-1,3,5-triazine and benzoyl peroxide are mixed with ethyl acetate in a mass ratio of 90:5:8:5:0.5:150, and the mixture is heated to 70° C. in a nitrogen atmosphere and polymerized for 3 hours to obtain the product.
[0045] Example 2
[0046] A method for preparing an acrylic foam tape comprises the following steps:
[0047] The modified polyacrylate masterbatch, hollow glass microspheres, isocyanate curing agent, nonionic polymer block copolymer, rosin-based resin, carbon black and ethyl acetate are mixed in a mass ratio of 65:2.5:0.8:0.5:2:3:45 and coated on a PET release film with a coating thickness of 100 μm. The mixture is heated and dried to remove the solvent.
[0048] The preparation method of the modified polyacrylate masterbatch comprises the following steps:
[0049] n-Butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, 2-vinyl-4,6-dimethyl-1,3,5-triazine and benzoyl peroxide are mixed with ethyl acetate in a mass ratio of 90:5:8:5:0.5:150, and the mixture is heated to 70° C. in a nitrogen atmosphere and polymerized for 3 hours to obtain the product.
[0050] Example 3
[0051] A method for preparing an acrylic foam tape comprises the following steps:
[0052] The modified polyacrylate masterbatch, hollow glass microspheres, isocyanate curing agent, nonionic polymer block copolymer, rosin-based resin, carbon black and ethyl acetate are mixed in a mass ratio of 65:2.5:0.8:0.5:2:3:45 and coated on a PET release film with a coating thickness of 100 μm. The mixture is heated and dried to remove the solvent.
[0053] The preparation method of the modified polyacrylate masterbatch comprises the following steps:
[0054] n-Butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, 4-vinyl-6-phenyl-1,3,5-triazine-2-amine and benzoyl peroxide are mixed with ethyl acetate in a mass ratio of 90:5:8:5:0.5:150, and the mixture is heated to 70° C. under a nitrogen atmosphere and polymerized for 3 hours to obtain the product.
[0055] Example 4
[0056] A method for preparing an acrylic foam tape comprises the following steps:
[0057] The modified polyacrylate masterbatch, hollow glass microspheres, isocyanate curing agent, nonionic polymer block copolymer, rosin-based resin, carbon black and ethyl acetate are mixed in a mass ratio of 65:2.5:0.8:0.5:2:3:45 and coated on a PET release film with a coating thickness of 100 μm. The mixture is heated and dried to remove the solvent.
[0058] The preparation method of the modified polyacrylate masterbatch comprises the following steps:
[0059] n-Butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, 1-phenyl-2-propenylbenzene and benzoyl peroxide are mixed with ethyl acetate in a mass ratio of 90:5:8:5:0.5:150, and the mixture is heated to 70° C. under a nitrogen atmosphere and polymerized for 3 hours to obtain the product.
[0060] Example 5
[0061] The same as Example 1, the only difference is that the mass ratio of n-butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, 2-vinyl-4,6-diphenyl-1,3,5-triazine and benzoyl peroxide to ethyl acetate is 90:5:8:3:0.5:150.
[0062] Example 6
[0063] The same as Example 1, the only difference is that the mass ratio of n-butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, 2-vinyl-4,6-diphenyl-1,3,5-triazine and benzoyl peroxide to ethyl acetate is 90:5:8:7:0.5:150.
[0064] Test Example 1
[0065] The acrylic foam tape obtained in the control example and the embodiment was subjected to impact resistance test, including point impact test and surface impact test, wherein the point impact test is to take a 30g steel ball, drop it from a height of 10cm to obtain a blank test value V1, then lay the sample to be tested on the surface, drop the same small ball from the same height, obtain the test value V2, and the point impact energy absorption rate is (V1-V2) / V1*100%, and each sample is tested 3 times to obtain the average value. The surface impact test method is to place a 0.7mm glass on the platform surface, drop a 30g steel ball from a height of 10cm, obtain a blank test value V1, then lay a 40mm*30mm sample on the glass surface, place the sample to be tested downward on the platform surface, drop the same small ball from the same height, obtain the test value V2, and the surface impact energy absorption rate is (V1-V2) / V1*100%, and each sample is tested 3 times to obtain the average value.
[0066] Table 1 Impact test results of acrylic foam tape
[0067] Experimental protocol Tape thickness / μm Point impact / % Surface impact / % Comparative Example 1 100 50 45 Example 1 100 63 58 Example 2 100 55 51 Example 3 100 53 50 Example 4 100 51 49 Example 5 100 56 51 Example 6 100 68 59
[0068] Acrylic foam, as a buffer material with good resilience, can be applied to the display module of electronic equipment. It has excellent protection, sealing and gap filling properties, and the foam itself has unique self-adhesiveness. Acrylic foam is prepared by adding glass hollow microspheres to form a porous structure, which has high elasticity and is not prone to irreversible deformation under conditions of large compression ratio. Acrylate masterbatch can make the foam have good impact resistance. However, compared with the embodiment, the control example 1 does not add additional modified monomers, so the impact resistance is poor. This may be because the modified monomers added in the embodiment have rigid structures such as heterocyclic rings or benzene rings, so the mechanical properties of the obtained polyacrylate are better. Compared with embodiments 2 to 4, the modified monomers in embodiment 1 have both heterocyclic rings and benzene rings, so the structural rigidity of the polyacrylate finally obtained is stronger, the configuration is more stable, and therefore the performance is the best. Compared with embodiments 5 to 6, when the content of the modified monomer in embodiment 1 increases, the crosslinking density and cohesion of the polyacrylate will increase accordingly, so the impact resistance is better.
[0069] Test Example 2
[0070] The acrylic foam tapes prepared in the control example and the example were tested for 180° peel strength according to GB / T2792-2014 "Test method for peel strength of adhesive tape". Samples were prepared according to the peel strength test and placed in ovens at different temperatures for a period of time, then the samples were taken out and cooled to room temperature, and finally slowly peeled (180°) and observed to see if there was any residual adhesive to judge its excellent heat resistance.
[0071] Table 2 Adhesive performance and heat resistance test results of acrylic foam tape
[0072]
[0073] The main chain of acrylate is a saturated carbon-carbon structure and has certain heat resistance. However, due to the low crosslinking density after polymerization, the molecular chain is prone to relative movement in a high temperature environment, the cohesive strength and adhesive performance are significantly reduced, and the failure morphology after peeling is mainly cohesive failure, with more residual glue. Therefore, the tape sample in Control Example 1 exhibits poor heat resistance and low viscosity. In the embodiment, the modified polyacrylate is prepared by introducing a heat-resistant monomer. Since the heterocyclic ring and the aromatic ring have good thermal stability, the heat resistance of the final product can be greatly improved. Compared with Examples 2 to 4, Example 1 has both heterocyclic rings and benzene rings in the modified monomer, so the final polyacrylate has stronger structural rigidity and more stable configuration. Compared with Examples 5 to 6, when the content of the modified monomer in Example 1 increases, although the crosslinking degree and cohesion will increase, the adhesion will also decrease at the same time, and the peel strength will be affected. Therefore, Example 1 is relatively the best.
[0074] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for preparing an acrylic foam tape, characterized in that: The steps include: The modified polyacrylate masterbatch, foamed microspheres, curing agent, dispersant, tackifier, filler and solvent are mixed and coated on the release film, and then heated and dried to remove the solvent; The preparation method of the modified polyacrylate masterbatch comprises the following steps: n-Butyl acrylate, acrylic acid, 2-ethylhexyl acrylate, 2-vinyl-4,6-diphenyl-1,3,5-triazine and benzoyl peroxide are mixed with ethyl acetate in a mass ratio of 80-100:2-5:5-10:2-8:0.1-0.5:100-200, and the mixture is heated to 65-80°C in a nitrogen atmosphere and polymerized for 2-3 hours to obtain the product; The mass ratio of the modified polyacrylate masterbatch, the foamed microspheres, the curing agent, the dispersant, the tackifier, the filler and the solvent is 50-80:1-3:0.5-2:0.1-1:1-5:2-5:10-50.
2. The method for preparing the acrylic foam tape according to claim 1, characterized in that: The foamed microspheres are hollow glass microspheres.
3. The method for preparing the acrylic foam tape according to claim 1, characterized in that: The curing agent is one of an isocyanate curing agent, an epoxy curing agent, and a pyridine curing agent.
4. The method for preparing the acrylic foam tape according to claim 1, characterized in that: The dispersant is one of a condensate of fatty alcohol and ethylene oxide, sodium polyacrylate, and a nonionic high molecular block copolymer.
5. The method for preparing the acrylic foam tape according to claim 1, characterized in that: The tackifier is a rosin-based resin.
6. The method for preparing the acrylic foam tape according to claim 1, characterized in that: The filler is carbon black; the solvent is one of dimethyl carbonate, ethyl acetate and toluene.
7. The method for preparing the acrylic foam tape according to claim 1, characterized in that: The coating thickness is 50-150 μm.
8. An acrylic foam tape, characterized in that: Prepared by the method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Stain-resistant acrylic foam tape and preparation method thereof
CN111548754A
Acrylic foam tape composition and method for preparing acrylic foam tape composition
CN106674417A
Polyacrylate, acrylic foam composition, acrylic foam adhesive tape as well as preparation methods and applications thereof
CN111072847A
Acrylic foam tape resistant to high-temperature and high-humidity environment and preparation method of acrylic foam tape