A high-frequency and high-speed circuit board blind hole manufacturing process

Through step-by-step drilling and multiple copper deposit electroplating treatments, the problem of difficult to ensure cross-blind hole accuracy and copper deposit quality in traditional processes is solved, and high-precision and high-efficiency cross-blind hole processing is achieved, which improves high-frequency circuit boards electrical performance and interconnect reliability.

CN118413953BActive Publication Date: 2024-11-01SICHUAN LONGYU TIANLING ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410866105.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-01
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

The traditional cross-blind hole production process is difficult to achieve precise depth and position control, resulting in electrical performance and reliability problems, and the quality of copper deposited electroplating is difficult to ensure, affecting interconnection reliability.

Method used

Using step-by-step drilling, batch pressing, chemical copper deposition and electroplating, the intermediate core plate is formed by vacuum hot pressing, and the first mechanical drilling and copper deposition treatment is carried out to form a through-type conductive through hole, and then X is performed. Ray positioning and secondary drilling of CNC machine tools form a stepped cross-blind hole structure, and multiple copper deposits and electroplating treatments are carried out to ensure the density and uniformity of the conductive layer.

Benefits of technology

It realizes high-precision, high-quality and high-efficiency cross-blind hole processing, significantly improves processing accuracy and electrical performance, ensures impedance matching and interconnection reliability of signal transmission, and improves the performance and stability of high-frequency circuit boards.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of high-frequency and high-speed printed circuit board manufacturing, and in particular to a high-frequency and high-speed circuit board blind hole manufacturing process, which comprehensively uses multiple key technologies such as step-by-step mechanical drilling, batch vacuum lamination, plasma surface treatment, and optimized copper electroplating. By precisely controlling the blind hole forming, a stepped transition structure is formed between adjacent vias, and an optimized electroplating process is used to achieve a copper layer thickness uniformity of more than 90% in the blind hole. In terms of performance indicators such as high-frequency transmission and reliability, the high-frequency circuit board manufactured by the new process has significant advantages over conventional process products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high-frequency and high-speed printed circuit board manufacturing, and in particular to a process for manufacturing blind holes of high-frequency and high-speed printed circuit boards. Background Art

[0002] With the rapid development of modern electronic information technology, high-frequency and high-speed circuit boards have become indispensable key components in the fields of communications, computers, aerospace, etc. High-frequency and high-speed circuit boards need to support higher signal frequencies and data transmission rates, while requiring higher integration, smaller size, and better reliability. In order to meet these requirements, the design and manufacturing technology of high-frequency and high-speed circuit boards are developing towards higher density and more refinement.

[0003] Cross blind vias refer to two adjacent blind vias in the inner layer of a circuit board. Their positions are staggered to form a conductive path that crosses each other. Compared with ordinary blind vias, cross blind vias can achieve more flexible and higher-density wiring design, greatly improving the integration and wiring efficiency of circuit boards. In high-frequency and high-speed circuit boards, the reasonable use of cross blind via structures can effectively shorten the transmission path of key signals, reduce transmission loss and delay, and thus improve the high-frequency performance and signal integrity of the system.

[0004] In addition, cross blind vias are also an important carrier for high-density component assembly. By forming pads in cross blind vias, direct assembly of IC chips, passive components, etc. can be achieved, thereby simplifying wiring design and reducing interconnection complexity. Especially for high-density packaging forms such as BGA and CSP, the use of cross blind vias can significantly improve assembly density and reliability. Compared with conventional through-hole assembly, cross blind via assembly can reduce the pad size and reduce the occupation of circuit board wiring resources, while also improving the heat dissipation performance and mechanical strength of components.

[0005] However, the processing and manufacturing of cross blind vias also faces many technical difficulties. Due to the complex structure of cross blind vias and the stacking combination of multilayer board materials, traditional mechanical drilling processes are difficult to achieve precise depth control and position alignment. In addition, there are often irregular structures such as sharp corners and steps in cross blind vias, which also puts higher requirements on subsequent metallization treatment. How to improve the processing efficiency and yield rate of cross blind vias while ensuring dimensional accuracy and interconnection reliability is a key issue that needs to be urgently solved in the field of high-frequency and high-speed circuit board manufacturing.

[0006] In the conventional PCB cross blind via production process, a one-time drilling method is usually used to form deep cross blind vias. That is, using CNC mechanical drilling or laser drilling equipment, according to the design requirements, a cross blind via structure is drilled in the inner layer of the PCB at one time. Although this method is relatively simple to operate, there are often many problems in actual production, which makes it difficult to ensure processing quality and efficiency.

[0007] There are differences in the interlayer bonding strength and thermal expansion coefficient of multilayer circuit board materials, which can easily cause defects such as interlayer separation and tearing during the drilling process. This problem is particularly prominent when the one-time drilling depth is large. The vibration and heat generated by the drill bit during the cutting process will cause the fragile interlayer interface to bear greater stress, leading to delamination failure. At the same time, interlayer separation will also increase the roughness of the hole wall and tear the copper foil, burying hidden dangers for subsequent metallization processing.

[0008] The drilling process of deep cross blind holes is complicated and can easily cause hole position deviation and dimensional error. When processing deeper blind holes, the drill bit is prone to deflection and bending, causing the actual axis of the hole to deviate from the designed position. Especially in the cross blind hole structure, the positions of adjacent blind holes are staggered. The deviation during the drilling process can cause the blind holes to be connected or misaligned, seriously affecting the electrical performance. In addition, when drilling deep blind holes, due to cutting force and difficulty in chip removal, the hole size is prone to change, and defects such as burrs and fiber protrusions are also prone to occur on the bottom and side walls of the hole.

[0009] The deep cross blind holes formed by one-time drilling have a large ratio of hole depth to hole diameter, which brings difficulties to the selection of tools and the optimization of cutting parameters. Conventional twist drills can hardly meet the requirements of blind hole processing with a large depth-to-width ratio, and micro-diameter drills have problems such as insufficient rigidity and easy breakage. Cutting parameters such as spindle speed and feed rate also need to be finely controlled, otherwise it is easy to cause quality defects such as hole wall damage and edge collapse. In short, the one-time drilling of deep cross blind holes is difficult and has high quality risks, which limits the improvement of production efficiency and yield rate.

[0010] The quality of copper deposition and electroplating of deep cross blind holes is difficult to guarantee. After forming the deep cross blind holes, chemical copper deposition and electroplating processes are required to form a conductive metal layer on the hole wall to achieve reliable electrical interconnection. However, for the deep cross blind holes formed by one-time drilling, their complex hole structure and aspect ratio characteristics bring many challenges to the copper deposition and electroplating processes, making it difficult to guarantee the quality of interconnection.

[0011] There are irregular structures such as sharp corners, blind ends, and steps inside deep cross blind holes, which hinder the full exchange and diffusion of chemical solutions and electroplating solutions. In the deep and narrow areas of the holes, the chemical solution is not updated smoothly, and bubbles are easily trapped, resulting in incomplete chemical reactions and poor density and uniformity of the deposited layer. Poor copper deposition not only affects the conductivity, but also causes defects such as pinholes and pitting during the subsequent electroplating process. In addition, surface defects such as rough inner walls of blind holes and exposed fibers will also reduce the adhesion and continuity of the copper layer.

[0012] The deep inner cavity of the deep cross blind hole is deep, which greatly prolongs the copper deposition and electroplating process. The extended chemical immersion time will intensify the interface reaction between the substrate and the copper layer, causing pinholes, blistering and other adverse effects. Excessive electroplating time will also lead to increased stress in the copper layer, coarsening of the crystal grain size, and other problems, which will lead to cracking of the hole wall and deterioration of the conductive performance. Therefore, how to achieve high-quality and efficient copper deposition and electroplating for the deep cross blind hole structure is the key to ensuring the reliability of interconnection.

[0013] The depth and position accuracy of cross blind vias are important factors affecting the performance of high-frequency and high-speed circuit boards. However, the depth and position of cross blind vias processed under conventional processes are often difficult to accurately control, which in turn causes a series of electrical performance and reliability issues.

[0014] For example, the depth deviation of the cross blind vias can cause impedance discontinuity and signal reflection. In high-frequency signal transmission, the size and shape of the blind via structure directly affect the characteristic impedance of the transmission line. When the depths of adjacent blind vias are inconsistent, impedance discontinuities will be formed on the signal transmission path, causing partial signal reflections and resulting in reduced signal integrity. The reflected energy can also cause crosstalk, ringing and other problems, seriously affecting the performance and stability of high-frequency circuits.

[0015] It can be seen that the conventional cross blind via manufacturing process has many shortcomings and is difficult to meet the increasingly high performance requirements of high-frequency and high-speed circuit boards. One-time drilling is prone to cause quality defects such as aperture size error and hole position offset; the complex hole structure brings difficulties to the copper plating process and affects the interconnection reliability; the blind hole depth and position error will also cause impedance mismatch, signal crosstalk, stress concentration and other performance and reliability problems. Therefore, it is urgent to develop a new cross blind via manufacturing process to overcome the various limitations of conventional processes and achieve high-quality and high-reliability cross blind via processing in a precise and controllable manner. Summary of the invention

[0016] In view of the limitations of conventional circuit board cross blind hole production processes, the present invention proposes an innovative high-frequency and high-speed circuit board cross blind hole production method. This method cleverly utilizes multiple technologies such as step-by-step drilling, batch lamination, chemical copper deposition and electroplating to achieve high-precision, high-quality and high-efficiency cross blind hole processing, effectively overcoming the shortcomings of traditional processes.

[0017] The overall process of a high-frequency and high-speed circuit board cross blind via manufacturing process is as follows:

[0018] Prepare substrates, including several double-sided copper foil laminates and prepregs, and perform necessary surface treatments;

[0019] Stacking some double-sided copper foil laminates and prepregs according to design requirements, and pressing them by vacuum hot pressing to form an intermediate multi-layer core board;

[0020] Performing the first mechanical drilling on the middle multi-layer core board to form a through-type conductive through hole;

[0021] The middle multi-layer core board is subjected to copper deposition treatment, and a dense and uniform metal copper layer is deposited on the inner wall of the through hole by electroplating;

[0022] Apply a dry film on the surface of the middle multi-layer core board, and form a through-hole protective film by exposure and development;

[0023] The middle multi-layer core board is laminated for the second time with the remaining double-sided copper foil laminates and prepregs according to the design requirements, and is pressed again by vacuum hot pressing to form a complete multi-layer circuit board substrate;

[0024] X-ray positioning and CNC machine tools are used for secondary drilling to drill new conductive through holes on both sides of the existing through holes, and the drilling depth is less than the thickness of the substrate, forming a stepped cross blind hole structure;

[0025] The copper deposition treatment, hole wall insulation and metal copper electroplating are performed in sequence to form a cross blind hole conductive layer;

[0026] Finally, graphic transfer, etching, surface treatment, character marking and other processes are carried out to complete the processing and production of high-frequency and high-speed circuit boards.

[0027] Specifically,

[0028] The high-frequency and high-speed circuit copper-clad laminate substrates suitable for this process must have excellent dielectric properties and thermomechanical properties. The dielectric constant (Dk) of the substrate should be as low as possible, and materials with a Dk between 3.0 and 4.5 should be selected, such as Rogers RO4000 series, Taconic RF-35A, Panasonic Megtron 6, etc. The dielectric loss tangent (Df) of the substrate should also be small enough, generally requiring Df < 0.005.

[0029] The coefficient of thermal expansion (CTE) of the substrate should be close to that of the copper foil to reduce thermal stress and warping. The CTE of the FR-4 series substrate is relatively large and is no longer suitable for high-frequency and high-speed applications. The CTE of the high-frequency substrates such as Rogers and Taconic mentioned above is controlled at 10-20ppm / ℃.

[0030] The heat resistance (Td) and moisture resistance of the substrate are also critical. Td needs to be higher than the highest process temperature and should be above 260°C. The moisture absorption rate should be lower than 0.1% to avoid defects such as delamination and blistering under high temperature and humidity.

[0031] The selection of substrate copper foil is crucial for copper electroplating. In the new process, low profile (L / L), ultra-low profile (V / L) or ultra-low profile (X / L) electrolytic copper foil is selected, and its surface roughness Ra is controlled below 0.5μm, which is conducive to the formation of a dense, uniform, and highly adhesive porous copper deposition layer. The thickness of the copper foil is mainly 18μm and 35μm. Under special requirements, 9μm or 70μm thick copper foil can be selected.

[0032] In order to improve the bonding strength between the copper foil and the substrate and improve the wettability between the substrate surface and the hole wall, the substrate surface needs to be treated before lamination. Commonly used surface treatment methods are micro-etching and plasma etching.

[0033] Micro-etching treatment uses a mixture of sodium persulfate (80-100g / L) and sulfuric acid (50-80g / L) to soak the substrate at 30-40℃ for 60-120s to roughen the surface. After treatment, the bonding strength of the substrate can be increased by 20-50%.

[0034] Plasma etching treatment places the substrate in plasma and bombards the substrate surface with active gases such as oxygen or carbon tetrafluoride, removing the surface contamination layer while producing a certain degree of roughening. The process parameters are power 300-1000W, pressure 50-200Pa, and time 60-180s.

[0035] The micro-etching method has a low cost, but consumes a lot of chemicals, has a heavy burden on waste liquid treatment, and is prone to deep substrate damage; the plasma method is clean and environmentally friendly, and can achieve nanoscale roughening, but it is more expensive. The specific choice needs to take into account factors such as product performance requirements and cost budget.

[0036] First, several double-sided copper foil laminates with treated surfaces and prepregs (PP) are accurately assembled according to the stacking order of the product design. Prepregs are used as adhesives between the inner layers of the core board, and resin systems that are compatible with the laminate substrate, such as epoxy type, polyimide type, etc., need to be selected.

[0037] A vacuum hot press is used to apply heat pressure to each layer of the core board, so that the prepreg is fully melted and infiltrated into the laminate, forming a dense and reliable interlayer bond. The common process parameters of vacuum hot pressing are: temperature 180-210℃, pressure 0.5-2.0MPa, and holding time 60-120min. The constant temperature time and heating rate also need to be optimized according to the melting characteristics and thickness of PP. After the hot pressing, the core board is naturally cooled, and the cooling rate is controlled at 2-5℃ / min.

[0038] The laminated multi-layer core board is mechanically drilled for the first time, and conductive through holes are drilled at the corresponding positions of the inner and outer layers. Considering the balance between processing accuracy and cost, CNC mechanical drilling is mainly used, supplemented by laser drilling.

[0039] The drill bit is made of micro-particle cemented carbide material, with a diameter range of 0.1-0.3mm, a sharp angle of 130-140°, and 2-4 spiral grooves. The specific size needs to match the total thickness of the core plate and the aperture requirements. The laser uses a 355nm ultraviolet Nd:YAG laser, with a spot diameter of 20-50μm and a peak power of 10-20W.

[0040] To ensure the quality and efficiency of drilling, the setting of drilling parameters is crucial. The spindle speed is controlled at 80000-120000rpm, and the feed speed is 200-800mm / min. The retraction speed is 800-1,500mm / min, and a multi-step retraction strategy is adopted. The drilling and retraction speeds need to be adjusted according to the actual conditions of the substrate and the aperture. Generally, the smaller the aperture and the thicker the substrate, the higher the speed. High-quality water-based cutting fluid is used for cooling and lubrication throughout the process, and chips are removed in time.

[0041] The core board after mechanical drilling needs to be treated with chemical copper deposition and electroplating to form a fine conductive interconnection layer on the inner wall of the through hole. The copper deposition adopts the hot liquid method, with sodium hypophosphite as the reducing agent, and the immersion treatment is carried out at 60-70℃ for 20-30min. In order to improve the uniformity of the thickness of the deposited layer, it can be immersed in multiple times, each time for 10-15min.

[0042] After the copper deposition is completed, a copper sulfate electroplating solution is used to plate a dense and uniform copper layer on the hole wall. In addition to copper sulfate (220-250g / L) and sulfuric acid (60-80g / L), a small amount of additives such as brightener and leveler need to be added to the electroplating solution to control grain refinement and deposition uniformity. The electroplating is carried out at room temperature, the cathode current density is controlled at 2-3A / dm², and the electroplating is carried out for 30-60 minutes under stirring conditions to make the hole copper thickness reach 25-35μm.

[0043] The core board needs to be pre-treated before electroplating, including chemical degreasing, micro-etching, pickling activation, etc., to improve the bonding strength between the copper layer and the substrate. After electroplating, the core board needs to be post-treated, including water washing, drying, etc., and the hole copper thickness uniformity and conductivity are tested.

[0044] Using a vacuum hot pressing process similar to the previous one, the middle multi-layer core board is laminated with other surface-treated laminates and prepregs to form a complete multi-layer circuit board substrate. Due to the addition of a new lamination layer, the hot pressing parameters need to be adjusted appropriately. Common parameters are: temperature 190-220℃, pressure 0.5-2.5MPa, and holding time 90-180min. The cooling rate is controlled at 1-3℃ / min to reduce thermal stress.

[0045] After the lamination, the CNC machine tool is used to perform a second mechanical drilling on the multi-layer substrate to drill a via hole that penetrates the laminated structure. The diameter of the via hole is 0.3-0.8mm, depending on the circuit design requirements and wiring density.

[0046] The drilling parameters are similar to the above parameters, but due to the increase in the total thickness of the substrate, the feed speed needs to be appropriately reduced to 100-400mm / min, and the spindle speed needs to be reduced accordingly. The drill diameter also needs to be appropriately increased and the sharp angle adjusted accordingly.

[0047] In order to improve the drilling positioning accuracy, X-ray non-destructive testing and CCD alignment system are used to achieve accurate alignment between the drill hole and the inner layer circuit and blind buried hole, and the position deviation is controlled within ±20μm. At the same time, the drill bit wear state must be strictly controlled, the drill bit performance is monitored through the online detection system, and the drill bit is replaced in time.

[0048] After the vias are drilled, a layer of insulating material is coated on the hole wall using vacuum-assisted perforation resin coating technology. The material is epoxy resin or polyimide resin, etc., and auxiliary materials such as curing agent and pigment are added. The coating process is carried out under vacuum conditions so that the resin can fully infiltrate the hole wall and fill the pores. The coated substrate is cured in an oven at a curing temperature of 130-170°C for 30-60 minutes.

[0049] Based on the resin insulation layer coated on the hole wall, copper deposition and copper electroplating are performed again to form a new conductive interconnection layer on the inner wall of the via hole and interconnect with the existing circuit. The copper deposition and electroplating process parameters are basically the same as the above parameters, but they need to be appropriately adjusted according to the hole diameter, hole depth and substrate characteristics.

[0050] On the basis of the conductive vias, a two-step controlled deep drilling process is used to form a stepped cross blind hole structure between adjacent vias. First, the first blind hole is drilled at the edge of the via using CNC equipment and precision tools, and its depth is slightly less than the total thickness of the substrate. The tool diameter is 20-50μm smaller than the via to avoid cutting through the substrate.

[0051] After completing the first blind hole, the tool is offset a certain distance (20-100μm) in the XY plane, and the Z-direction feed depth is adjusted to drill the second blind hole at the edge of the adjacent via hole. The depth difference between the two blind holes is controlled at 20-50μm to form a stepped transition zone to suppress impedance discontinuity.

[0052] Both drilling steps use lower feed speeds (50-200mm / min) and spindle speeds (50,000-80,000rpm) to reduce cutting forces and thermal effects. At the same time, the drill bits are coated with special coatings (such as diamond coatings) to improve wear resistance and machining accuracy. Online measurement and servo feedback systems are also introduced into the drilling cycle to monitor the hole depth in real time and dynamically adjust the drilling parameters. The depth control accuracy is within ±5μm.

[0053] The drilled cross blind hole structure is copper plated and electroplated to form a reliable conductive interconnection on the inner wall of the blind hole. Since the blind hole depth is small (<0.1mm) and the hole diameter is also small (0.1-0.2mm), the deposition difficulty is greatly reduced.

[0054] To further improve the quality and uniformity of copper deposition in blind holes, the copper salt concentration and pH value can be increased, the amount of EDTA and reducing agent can be reduced, and appropriate stirring can be used on the basis of the conventional copper deposition solution formula. The additive ratio can be optimized during electroplating, and special processes such as pulse electroplating and periodic reversal current can be used to make the copper grains in the blind holes smaller and denser, and the deposition more uniform and smooth.

[0055] At the same time, after copper deposition, the inner wall of the blind hole can be micro-etched to remove a very thin layer of copper to expose the fresh copper surface, which helps to improve the bonding strength between the subsequent electroplated copper and chemical copper. During the electroplating process, the cathode plate needs to be stirred to promote the exchange and renewal of the electrolyte in the blind hole.

[0056] After the optimized copper electroplating process, the copper deposited layer in the blind hole is dense and uniform, the thickness deviation is controlled within 10%, and the bonding force with the hole wall is greater than 10N / cm. This not only ensures the conductivity and reliability of the blind hole interconnection, but also creates favorable conditions for subsequent surface fine processing.

[0057] The process of forming conductive patterns on both sides of a multilayer board mainly includes: coating photoresist, exposure and development, pattern transfer, rapid etching, etc. The photoresist needs to be a photosensitive dry film with high resolution and strong adhesion. When coating, pay attention to uniform thickness and no bubbles.

[0058] The exposure is done with a high-precision exposure machine, and a cold light source with good collimation is preferred. The exposure energy density is controlled at 100-200mJ / cm². The substrate covered with dry film is tightly attached to the graphic film to ensure that there is no offset or bubbles. After exposure, spray development is used, and the development time is 40-60s.

[0059] Etching is done with copper sulfamate etching solution at 45-55°C for rapid etching, and the etching time is controlled at 60-90s. After etching, wash with water in time, and remove the film with warm water containing surfactant, and check the pattern integrity and line width at the same time.

[0060] In order to improve the anti-oxidation performance, solderability and appearance quality of the circuit board, it is necessary to carry out fine processing on the surface conductive pattern. Commonly used surface treatment methods include tin spraying, immersion gold, chemical nickel gold, etc.

[0061] The tin spraying treatment forms a dense and uniform pure tin layer on the surface of the substrate, and its thickness is controlled at 0.8-1.2μm. The tin spraying adopts the lead-free tin spraying process, the tin liquid temperature is 240-260℃, the spraying speed is 1.5-2.5m / min, and the air pressure is 0.05-0.06MPa. After spraying, deionized water is used to remove slag in time and trimming is carried out.

[0062] The gold-plating process can obtain a gold-plated surface with better corrosion resistance. Before gold-plating, the substrate needs to be treated with acid pickling, water washing, micro-etching, nickel plating, and gold immersion in sequence. The chemical nickel bath adopts sodium hypophosphite type, and is deposited at 85-90℃ for 4-6 minutes to obtain a dense alloyed nickel layer. Gold immersion is carried out in a neutral thiourea gold salt solution, soaking at 85-95℃ for 3-5 minutes, and the thickness of the gold layer reaches 0.05-0.1μm.

[0063] The chemical nickel-gold process is more suitable for occasions with higher requirements for solderability and corrosion resistance. Its process includes degreasing, microetching, pre-wetting, chemical nickel plating, chemical immersion gold, anti-oxidation and other steps. Nickel plating and immersion gold are carried out at 90-95℃ and 85-90℃ respectively, and the time is 20-30min. The total thickness of the nickel-gold layer is controlled at 4-6μm.

[0064] The character screen printing on the surface of the circuit board is very important for product identification and assembly guidance. Using photosensitive polymer relief printing or inkjet printing can obtain clear and durable identification patterns.

[0065] The production of photosensitive polymer relief plates adopts thick film photolithography process. After coating, exposure, development, curing after exposure, etc., relief characters are formed on the surface of the plate. Then the ink is transferred to the product surface by pad printing or roller printing. In order to improve the transfer rate, the viscosity of the ink and the relief plate material need to be optimized. At the same time, the ink curing is strengthened, and a combination of UV light curing or hot air drying is used.

[0066] Inkjet printing uses digital inkjet printing equipment to directly print the pattern to be printed on the product surface. Inkjet inks must have excellent color saturation and adhesion. Printing accuracy requires nozzle diameter of 30-50μm, drive frequency of 30-50kHz, and positioning accuracy of ±10μm. The printing speed depends on the size and complexity of the pattern, generally 0.2-1.0m / s. The printed characters can be cured by UV light for 20-30s to achieve a durable and firm effect.

[0067] Through the above series of refined processing steps, the processing and production of high-frequency and high-speed circuit boards are completed. The multilayer board forms a fine conductive pattern on the surface, completing the SMT pads required for component assembly; the board surface is covered with a reliable protective coating, which has excellent anti-oxidation performance and solderability; the standardized product logo is clearly printed, laying the foundation for the subsequent process connection. DETAILED DESCRIPTION

[0068] In order to more intuitively demonstrate the application effect of the new high-frequency and high-speed circuit board cross blind hole manufacturing process, the high-frequency circuit board for 5G base stations is taken as an example to describe its entire processing and manufacturing process in detail.

[0069] The high-frequency circuit board in this example uses Rogers RO4003C high-frequency copper-clad laminate as the substrate, with a dielectric constant of Dk = 3.38 and a dielectric loss of Df = 0.0027 (10GHz), which meets the requirements of 5G high-frequency applications. The substrate adopts a standard size of 18″×24″, with three thicknesses of 8mil, 20mil and 40mil, which are used to make the signal layer, ground layer and power layer respectively.

[0070] The copper foil is Mitsui VLP-18 electrolytic copper foil with a thickness of 18μm and a roughness of Ra = 0.3μm after roughening treatment. The prepreg is Rogers RO4450F prepreg with a Dk matching the substrate and a thickness of 3mil.

[0071] The substrate was cut into the required size and dust was removed. The substrate and PP surface were treated using a Japanese Samco PD-360ST plasma etcher with a power of 600 W, a pressure of 100 Pa, a gas ratio of O2:CF4=4:1, and a treatment time of 90 s.

[0072] The surface treated RO4003C substrate and RO4450F prepreg are alternately stacked to form a symmetrical core board structure. The signal layer is 2×8mil substrate + 1×3mil PP, and the power / ground layer is 2×40mil substrate + 3×3mil PP.

[0073] The core panels were laminated using a Lauffer ZXVH-170 vacuum hot press with a vacuum degree of 0.1 Pa, a pressure of 190°C / 600 kPa for 60 min, and demoulding after cooling to <80°C. The cooling rate was 3°C / min.

[0074] The inner layer circuits of the two types of core boards after lamination were processed separately. Orbotech Paragon-8800i fully automatic circuit imaging machine was used, with a resolution of 25400dpi and an alignment accuracy of ±12μm. The minimum line width and line spacing of the inner layer can reach 50μm / 50μm. The etching used a sulfuric acid hydrogen peroxide system, spray etching for 60s, and the etching factor was controlled at 2.5-3.0. After stripping, browning, development and other surface treatments were performed.

[0075] The core board with the inner layer circuit is CNC machine drilled. A Schmoll Rapid-2030 drilling machine is used, with a maximum spindle speed of 180,000 rpm and a hole diameter range of 0.1-3.2 mm. According to the design requirements, conductive through holes are drilled at the corresponding positions of the inner layer board, with a hole diameter of 0.20 mm.

[0076] The ultra-fine carbide drill with a diameter of 0.20mm has a feed speed of 500mm / min, a spindle speed of 120000rpm, a special composite pad, a retraction speed of 1000mm / min, and a retraction every 400μm. High-quality water-based cutting fluid is used for cooling throughout the process, and high-pressure chip blowing is used.

[0077] The drilled plate was subjected to chemical degreasing, soft etching, water washing, micro-etching, pre-wetting and other treatments in turn, and then chemical copper deposition was carried out using the HCHO method. The liquid temperature was 60°C, the pH value was 12.8, and it was immersed twice under stirring conditions, each time for 15 minutes, so that the hole copper thickness reached 1.0μm.

[0078] The copper-plated plate is placed in a copper sulfate electroplating solution with a cathode current density of 2.5A / dm² and electroplating for 50 minutes to make the hole copper thickness reach 30μm. The current is reversed periodically, with a forward direction of 40s and a reverse direction of 5s. High-quality additives are added to the electroplating solution to improve the density and uniformity of the copper layer.

[0079] The signal layer and power / ground layer core board after copper plating are micro-etched on the surface and insulated by browning method, and then laminated with other new substrates and PP in the order of signal layer, ground layer, and power layer. The lamination temperature and pressure are 200℃ and 900kPa respectively, and the pressure holding time is 90min.

[0080] X-ray positioning was performed on the laminated multilayer board, and a Schmoll Rapid-2030 drilling machine was used to drill 0.30 mm via holes at the corresponding positions. The drill speed was 100,000 rpm and the feed speed was 300 mm / min.

[0081] After drilling, the inner wall of the hole was plasma etched at a power of 300 W for 60 seconds to roughen the hole wall. Then, a polyimide film insulation layer was coated using vacuum-assisted perforation technology, and the curing conditions were 160°C / 45 minutes. Chemical copper deposition and electroplating were performed again, with process parameters similar to those mentioned above, so that the thickness of the conductive layer reached 25 μm.

[0082] A Mitsubishi ML605GTi CO2 laser drilling machine was used to form stepped cross blind holes on both sides of the conductive through hole. The first step of drilling was 0.15mm in diameter and 0.58mm in depth; after an offset of 50μm, the second step of drilling was 0.15mm in diameter and 0.53mm in depth. The depth difference between the two holes was controlled at 50±5μm.

[0083] The laser parameters for two-step drilling are: wavelength 10.6μm, power 15W, frequency 5kHz, pulse width 60ns, spot diameter 50μm, scanning speed 200mm / s. During the drilling process, the machine vision monitors the hole depth in real time, and the servo system adjusts the drilling parameters in real time.

[0084] The vacuum-assisted pulse electroplating process is used for the laser blind hole. First, copper sulfate electroplating solution containing propiolic acid additives is used for electroplating at a current density of 1.5A / dm² for 60 minutes, and then copper sulfate solution without additives is used for electroplating at 3A / dm² for 30 minutes. After multiple pulse cycles, the copper thickness of the blind hole reaches 25μm, and the thickness uniformity is better than 90%.

[0085] The multilayer board with the completed step blind hole is patterned and etched. The solder mask ink is first printed by a fully automatic screen printer to protect the metal surface, and then UV exposure is performed. The etching uses sulfuric acid hydrogen peroxide solution, spray etching at 50°C for 60s. After stripping, the line width accuracy is tested, and the deviation is <5μm.

[0086] The etched board surface is treated with chemical nickel-gold process, first degreasing and activating in low pH sulfuric acid electrolyte for 5s, then chemically plating nickel in medium phosphorus sodium hypophosphite plating solution for 30min, with a nickel layer thickness of 5-7μm; then displacing gold in weak acid thiourea gold salt solution for 5min, with a gold layer thickness of 0.08-0.12μm. After deposition, an antioxidant is applied and dried.

[0087] The character logo is printed by a fully automatic platform screen printer with a printing accuracy of ±15μm. Black quick-drying epoxy ink is used, UV curing, power 80W, curing time 10s. The character line width reaches 80μm, and the adhesion reaches 4B level. After the character printing, the circuit board is V-Cut, profile milling, FQC inspection and sorting are completed.

[0088] The key structural parameters of the 5G high-frequency circuit board processed by the above process are as follows: minimum line width / line spacing 50μm / 50μm, copper thickness in the step blind hole 25μm, blind hole diameter 0.15mm, depth 0.53mm and 0.58mm, and the depth difference between the two holes is 50±5μm.

[0089] From the processing parameters, it can be seen that the new process uses a number of advanced technologies and equipment such as laser drilling, plasma etching, and vacuum-assisted electroplating, and achieves a high-precision step blind hole structure through precision control. The selection of high-frequency substrates and surface treatment processes also ensures excellent high-frequency electrical performance.

[0090] The processed high-frequency circuit boards were subjected to comprehensive performance tests and reliability tests. High-frequency transmission insertion loss < 0.3dB / inch (20GHz), phase delay variation < ±3ps (20GHz), impedance deviation < ±5%, far better than the 5G device index requirements.

[0091] After 1000 times of thermal shock (-45℃ / 15min~125℃ / 15min) and 500 hours of high temperature and high humidity (85℃ / 85%RH) tests, the drift of key electrical parameters is less than 2%, and the stepped blind hole structure is intact.

[0092] The high-frequency circuit board has been applied to the 5G base station remote radio unit (RRU) of a communications equipment manufacturer and has passed rigorous whole-machine testing. The 5G base station RRU using the high-frequency circuit board has increased its transmission power by more than 2dB, improved its receiving sensitivity by more than 3dB, and improved its EVM performance by more than 30%. This fully demonstrates the excellent comprehensive performance of the new process and the high-frequency and high-speed circuit board it manufactures.

[0093] The above examples demonstrate in detail the successful application of the new high-frequency and high-speed circuit board cross blind hole production process proposed in the present invention in the manufacture of 5G high-frequency circuit boards.

[0094] The beneficial technical effects of the present invention include the blind hole processing accuracy, electrical performance, interconnection reliability and other aspects, especially the innovative step-type controlled depth drilling method. The step-cross blind hole precisely formed by the new process can significantly reduce the high-frequency signal transmission loss, thereby improving the key indicators of the circuit board such as the rate-bandwidth product and signal-to-noise ratio. This is mainly due to two aspects. First, the high-precision blind hole forming greatly reduces the impedance discontinuity. Compared with the conventional "step"-shaped cross blind hole, the new process can obtain a smooth step transition zone. The finely controlled transition zone length (usually 0.5-2.0mm) and depth difference (usually 20-50μm) can achieve "impedance matching" of the signal in the transition zone. Second, the high conductivity, thickness uniformity and density of the copper layer deposited on the wall of the blind hole ensure excellent transmission characteristics. There is no substrate fiber residue on the inner wall of the mechanical blind hole, and a smooth copper layer can be obtained by chemical micro-etching and two-step deposition process. In addition, the new process significantly enhances the reliability of the interconnection structure through the optimization and coordination of many links such as substrate selection, hole forming, and copper deposition.

Claims

1. A method for making blind vias in a high-frequency and high-speed circuit board, characterized in that: The process of the method is as follows: Prepare a substrate, including a plurality of double-sided copper foil laminates and prepregs, and perform surface treatment, wherein the dielectric constant of the substrate is between 3.0 and 4.5, and the dielectric loss tangent is less than 0.005; Stacking some double-sided copper foil laminates and prepregs according to design requirements, and pressing them by vacuum hot pressing to form an intermediate multi-layer core board; Performing the first mechanical drilling on the middle multi-layer core board to form a through-hole; The middle multi-layer core board is subjected to copper deposition treatment, and a dense and uniform metal copper layer is deposited on the inner wall of the through hole by electroplating; Apply a dry film on the surface of the middle multi-layer core board, and form a through-hole protective film by exposure and development; The middle multi-layer core board is laminated for the second time with the remaining double-sided copper foil laminates and prepregs according to the design requirements, and is pressed again by vacuum hot pressing to form a complete multi-layer circuit board substrate; X-ray positioning and CNC machine tools are used for secondary drilling. New holes are drilled on both sides of the existing through holes, and the drilling depth is less than the thickness of the multi-layer circuit board substrate to form a stepped cross blind hole structure. Specifically, on the basis of the through hole, a two-step controlled depth drilling process is used to form a stepped cross blind hole structure between adjacent through holes. First, CNC equipment and precision tools are used to drill the first blind hole at the edge of the through hole. The depth is less than the total thickness of the multi-layer circuit board substrate. The tool diameter is 20-50μm smaller than the through hole. After completing the first blind hole, the tool is offset by 20-100μm in the XY plane. , and adjust the Z-direction feed depth to drill a second blind hole at the edge of the adjacent through hole. The depth difference between the two blind holes is controlled at 20-50μm to form a stepped transition zone to suppress impedance discontinuity; both steps of drilling use a feed speed of 50-200mm / min and a spindle speed of 50000-80000rpm to reduce cutting force and thermal effects. At the same time, the drill bits are all coated with diamond to improve wear resistance and machining accuracy; online measurement and servo feedback systems are also introduced into the drilling cycle to monitor the hole depth in real time and dynamically adjust the drilling parameters, with a depth control accuracy within ±5μm; The copper deposition treatment, hole wall insulation and metal copper electroplating are performed in sequence to form a cross blind hole conductive layer; Carry out graphic transfer, etching, surface treatment, and character marking processes to complete the processing and production of high-frequency and high-speed circuit boards.

2. The method according to claim 1, characterized in that The copper deposition treatment of the middle multi-layer core board and the deposition of a dense and uniform metal copper layer on the inner wall of the through hole by electroplating specifically include: chemical degreasing, soft etching, water washing, micro-etching, and pre-wetting treatment of the plate after drilling in sequence, and then chemical copper deposition by HCHO method, with a liquid temperature of 60°C and a pH value of 12.8, and immersion twice under stirring conditions, each time for 15 minutes, so that the hole copper thickness reaches 1.0 μm; placing the plate after copper deposition in a copper sulfate electroplating solution, with a cathode current density of 2.5A / dm², electroplating for 50 minutes, so that the hole copper thickness reaches 30 μm; using a periodic reversal current, 40 seconds in the forward direction and 5 seconds in the reverse direction; adding a brightener or a leveling agent to the electroplating solution to improve the density and uniformity of the copper layer.

3. The method according to claim 1, characterized in that The drilled cross blind hole structure is subjected to copper deposition and electroplating treatment to form conductive interconnection on the inner wall of the blind hole.

4. The method according to claim 1, characterized in that Carry out graphic transfer, etching, surface treatment, character identification process, complete the processing and production of high-frequency and high-speed circuit boards, including: first use a fully automatic screen printer to print solder mask ink to protect the metal surface, then perform ultraviolet exposure and development, use sulfuric acid and hydrogen peroxide solution for etching, spray etching at 50°C for 60s, test the line width accuracy after film removal, and the deviation is <5μm. The chemical nickel-gold process is used for the etched board surface, first degreasing and activating in a low-pH sulfuric acid electrolyte for 5s, and then chemically plating nickel in a medium-phosphorus sodium hypophosphite plating solution for 30min. The nickel layer is 5-7μm thick; then it is replaced with gold in a weakly acidic thiourea gold salt solution for 5 minutes, the gold layer thickness is 0.08-0.12μm, and after deposition, an antioxidant is applied and dried. A fully automatic platform screen printer is used to print character logos with a printing accuracy of ±15μm. Black quick-drying epoxy ink is used, UV curing, power 80W, and curing time 10s; the character line width reaches 80μm, and the adhesion reaches 4B level. After character printing, the circuit board is subjected to V-Cut board separation, shape milling, FQC inspection and sorting, and all processing is completed.