A polycarbonate alloy and a preparation method thereof
By hydroxylation treatment and thiol modification of nano silica, modified fillers are prepared, and the phase separation problem of polypropylene and bisphenol A polycarbonate is solved, and the mechanical properties of polycarbonate alloys are significantly improved, thus achieving the realization of Improved compatibility and mechanical performance.
Patent Information
- Application Number
- CN202410654506.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-05-24
AI Technical Summary
When blending polypropylene and bisphenol A polycarbonate, due to thermodynamic incompatibility, the mechanical properties are significantly lower than the linear sum value, and phase separation is prone to occur, and effective compatibilizers are lacking to improve the mechanical properties.
By hydroxylation of nano-silica and adding sulfhydryl silane coupling agent, thiol modification is performed, and then click reaction with long-chain olefins and glycidyl methacrylate under ultraviolet light, modifying fillers are prepared and polycarbonate is enhanced. Ester compatibility with polypropylene and improves mechanical properties.
The modified filler effectively improves the compatibility between polycarbonate and polypropylene, forms a polycarbonate alloy with excellent mechanical properties, avoids phase separation, and promotes the improvement of mechanical properties as a nano reinforcement material.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polycarbonate alloys, and in particular relates to a polycarbonate alloy and a preparation method thereof. Background Art
[0002] Polycarbonate is a thermoplastic engineering material containing a carbonate group in the molecular chain. It can usually be divided into various types such as aliphatic and aromatic. However, since only bisphenol A type polycarbonate can be industrially produced at present, polycarbonate mostly refers to bisphenol A polycarbonate, and polycarbonate alloy is a type of polymer material formed by blending bisphenol A polycarbonate with other polymers through non-chemical bonds. Among them, polypropylene is one of the typical representatives of polymers. Blending polypropylene with bisphenol A polycarbonate can improve and enhance the mechanical properties of bisphenol A polycarbonate. However, there are great differences between the two in structure. Polypropylene belongs to non-polar crystalline polymers, and polycarbonate belongs to polar non-crystalline polymers. At the same time, the two are also thermodynamically incompatible systems. This leads to the fact that if no compatibilizer is added when polypropylene and polycarbonate are blended, phase separation is very likely to occur. The mechanical properties after blending are significantly lower than the linear sum of the two. The improvement of mechanical properties becomes very limited, and there is still a lot of room for improvement. Summary of the invention
[0003] In view of the problems existing in the prior art, the purpose of the present invention is to provide a polycarbonate alloy and a preparation method thereof. The present invention creatively performs hydroxylation treatment on nano-silicon dioxide to generate more active hydroxyl groups on its surface, then adds a silane coupling agent with a mercapto group, realizes the mercapto modification of the nano-silicon dioxide through the condensation of alkoxy groups and hydroxyl groups, and finally adds long-chain olefins and glycidyl methacrylate in a certain weight ratio, and performs grafting-compounding of long-chain alkyl groups and epoxy groups based on mercapto-olefin click reaction under ultraviolet light irradiation, thereby obtaining a modified filler, so that the polycarbonate alloy formed after the modified filler and other components are blended can play a good volume expansion effect when actually used, the compatibility of polycarbonate and polypropylene is good, and the polycarbonate alloy has more excellent mechanical properties.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A polycarbonate alloy is prepared from polycarbonate, polypropylene and modified filler.
[0006] As a preferred technical solution of the present invention, the polycarbonate is directly purchased from the market.
[0007] As a preferred technical solution of the present invention, the polypropylene is directly purchased from the market.
[0008] As a preferred technical solution of the present invention, the modified filler is prepared by the following steps:
[0009] Step A: 20-30 parts by weight of anhydrous ethanol and 15-20 parts by weight of aqueous ammonia are stirred at room temperature for 5-10 minutes, then 5-8 parts by weight of nano-silicon dioxide are added, stirred at 35-50° C. for 1-2 hours, filtered, the filtrate is removed, washed with anhydrous ethanol, and finally vacuum dried at 60-80° C. until constant weight is obtained to obtain hydroxylated nano-silicon dioxide;
[0010] Step B: adding 1-2 parts by weight of deionized water and the hydroxylated nano-silica to 60-70 parts by weight of anhydrous ethanol, and then dropping 4-6 parts by weight of a mercaptosilane coupling agent at 40-50° C. while stirring, and continuing to stir at a constant temperature for 20-24 hours after the dropwise addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 60-80° C. until constant weight, to obtain mercapto-modified nano-silica;
[0011] Step C: Add the mercapto-modified nano-silica and 0.5-1 parts by weight of benzoin dimethyl ether to 50-60 parts by weight of anhydrous ethanol, stir and mix at room temperature for 5-10 minutes, then add 3-4 parts by weight of long-chain olefins and 2-3 parts by weight of glycidyl methacrylate, stir at 25-30° C. for 1-2 hours under ultraviolet light, filter, remove the filtrate, wash with anhydrous ethanol, and finally vacuum dry at 60-80° C. until constant weight, and the preparation is completed.
[0012] Furthermore, the mass fraction of the ammonia water in step A is 20-25%.
[0013] Furthermore, the particle size of the nano-silicon dioxide in step A is 20-50 nm.
[0014] Furthermore, the dripping rate in step B is controlled at 1-2 drops / s.
[0015] Furthermore, the mercaptosilane coupling agent in step B is at least one of γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane.
[0016] Furthermore, the long-chain olefin in step C is at least one of dodecene and 1-tetradecene.
[0017] Furthermore, the wavelength of the ultraviolet light in step C is 365nm.
[0018] As a preferred technical solution of the present invention, the amount of the polycarbonate used is 60-75 parts by weight.
[0019] As a preferred technical solution of the present invention, the amount of polypropylene used is 30-35 parts by weight.
[0020] As a preferred technical solution of the present invention, the amount of the modified filler is 8-10% of the sum of the weight of the polycarbonate and the polypropylene.
[0021] A method for preparing a polycarbonate alloy, the method comprising the following steps:
[0022] Step a: mixing polycarbonate, polypropylene and modified filler in a mixer for 10-15 minutes to obtain a mixed material;
[0023] Step b: adding the mixed material into a twin-screw extruder for extrusion granulation, and the preparation is completed.
[0024] Furthermore, the operating parameters of the twin-screw extruder in step b are as follows: the processing temperature is controlled at 220-250° C., the screw speed is controlled at 500-700 rpm, and the feed rate is controlled at 20-25 kg / h.
[0025] Beneficial effects of the present invention:
[0026] (1) The present invention creatively performs hydroxylation treatment on nano-silica to generate more active hydroxyl groups on its surface, then adds a silane coupling agent with a mercapto group, and realizes the mercapto modification of the nano-silica through the condensation of alkoxy and hydroxyl groups, and finally adds a certain weight ratio of long-chain olefins and glycidyl methacrylate, and carries out grafting-compounding of long-chain alkyl and epoxy groups based on mercapto-olefin click reaction under ultraviolet light, thereby obtaining a modified filler, so that the polycarbonate alloy formed after the modified filler and other components are blended can play a good role in increasing the volume when actually used, the compatibility of polycarbonate and polypropylene is good, and the polycarbonate alloy has more excellent mechanical properties.
[0027] (2) The present invention creatively uses nano-silicon dioxide as a basis and modifies its surface multiple times to prepare a modified filler, which can play a good volume expansion role when blended with polycarbonate and polypropylene. The obtained polycarbonate alloy has excellent mechanical properties. On the one hand, the surface of the modified filler is modified with a certain number of long-chain alkyl and epoxy groups. Since the long-chain alkyl is similar to polypropylene in structure and is a saturated hydrocarbon group, the modified filler has a very good affinity with polypropylene. At the same time, the surface of the modified filler is modified with epoxy groups, and the epoxy groups can be compatible with polycarbonate. The hydroxyl / carboxyl groups of the acid ester act to achieve the composite with polycarbonate. Moreover, since the adjacent group of the epoxy group is an ester group, the modified filler also has a certain affinity for polycarbonate that also contains a similar ester structure. Finally, through the amphiphilic nature of the modified filler, a bridging and volume-increasing effect is exerted to achieve the mutual fusion of polycarbonate and polypropylene, with good compatibility and no easy two-phase separation. The polycarbonate alloy has more excellent mechanical properties. On the other hand, the modified filler itself can also act as a nano-reinforcement material, which also plays a good role in promoting the mechanical properties of the polycarbonate alloy. DETAILED DESCRIPTION
[0028] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0029] The polycarbonate in all the embodiments and comparative examples of the present invention is purchased directly from the market, the manufacturer is LG Chemical, and the model is PC 1300-10; the polypropylene is purchased directly from the market, the manufacturer is Shanghai Petrochemical Co., Ltd., and the brand is PP T300; PP-g-GMA (glycidyl methacrylate grafted polypropylene) is purchased directly from the market, the effective active group is ≈1%, and the MFR (190°C / 2.16kg) is 70-100g / 10min.
[0030] Example 1
[0031] A polycarbonate alloy is prepared from polycarbonate, polypropylene and modified filler.
[0032] The polycarbonate was directly purchased from the market.
[0033] The polypropylene is directly purchased from the market.
[0034] The modified filler is prepared by the following steps:
[0035] Step A: 20 parts by weight of anhydrous ethanol and 15 parts by weight of aqueous ammonia are stirred at room temperature for 5 minutes, then 5 parts by weight of nano-silica are added, stirred at 35°C for 1 hour, filtered, the filtrate is removed, washed with anhydrous ethanol, and finally vacuum dried at 60°C until constant weight is obtained to obtain hydroxylated nano-silica;
[0036] Step B: adding 1 part by weight of deionized water and the hydroxylated nano-silica to 60 parts by weight of anhydrous ethanol, and then dropping 4 parts by weight of a mercaptosilane coupling agent at 40° C. while stirring, and continuing to stir at a constant temperature for 20 hours after the dropwise addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 60° C. until constant weight, to obtain mercapto-modified nano-silica;
[0037] Step C: Add the mercapto-modified nano-silica and 0.5 parts by weight of benzoin dimethyl ether to 50 parts by weight of anhydrous ethanol, stir and mix at room temperature for 5 minutes, then add 3 parts by weight of long-chain olefins and 2 parts by weight of glycidyl methacrylate, stir at 25°C for 1 hour under ultraviolet light, filter, remove the filtrate, wash with anhydrous ethanol, and finally vacuum dry at 60°C until constant weight, and the preparation is completed.
[0038] The mass fraction of the ammonia water in step A is 20%.
[0039] The particle size of the nano-silicon dioxide in step A is 20 nm.
[0040] The dropping rate in step B is controlled at 1 drop / s.
[0041] The mercaptosilane coupling agent in step B is γ-mercaptopropyltrimethoxysilane.
[0042] The long-chain olefin in step C is 1-tetradecene.
[0043] The wavelength of the ultraviolet light in step C is 365nm.
[0044] The polycarbonate is used in an amount of 60 parts by weight.
[0045] The amount of the polypropylene used is 30 parts by weight.
[0046] The modified filler is used in an amount of 8% of the total weight of the polycarbonate and the polypropylene.
[0047] A method for preparing a polycarbonate alloy, the method comprising the following steps:
[0048] Step a: mixing polycarbonate, polypropylene and modified filler in a mixer for 10 minutes to obtain a mixed material;
[0049] Step b: adding the mixed material into a twin-screw extruder for extrusion granulation, and the preparation is completed.
[0050] The operating parameters of the twin-screw extruder in step b are as follows: the processing temperature is controlled at 220° C., the screw speed is controlled at 500 rpm, and the feed rate is controlled at 20 kg / h.
[0051] Example 2
[0052] A polycarbonate alloy is prepared from polycarbonate, polypropylene and modified filler.
[0053] The polycarbonate was directly purchased from the market.
[0054] The polypropylene is directly purchased from the market.
[0055] The modified filler is prepared by the following steps:
[0056] Step A: 30 parts by weight of anhydrous ethanol and 20 parts by weight of aqueous ammonia are stirred at room temperature for 10 minutes, then 8 parts by weight of nano-silicon dioxide are added, stirred at 50° C. for 2 hours, filtered, the filtrate is removed, washed with anhydrous ethanol, and finally vacuum dried at 80° C. until constant weight is obtained to obtain hydroxylated nano-silicon dioxide;
[0057] Step B: adding 2 parts by weight of deionized water and the hydroxylated nano-silica to 70 parts by weight of anhydrous ethanol, and then dropping 6 parts by weight of a mercaptosilane coupling agent at 50° C. while stirring, and continuing to stir at a constant temperature for 24 hours after the dropwise addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 80° C. until constant weight, to obtain mercapto-modified nano-silica;
[0058] Step C: Add the mercapto-modified nano-silica and 1 part by weight of benzoin dimethyl ether to 60 parts by weight of anhydrous ethanol, stir and mix at room temperature for 10 minutes, then add 4 parts by weight of long-chain olefins and 3 parts by weight of glycidyl methacrylate, stir at 30° C. for 2 hours under ultraviolet light, filter, remove the filtrate, wash with anhydrous ethanol, and finally vacuum dry at 80° C. until constant weight, and the preparation is completed.
[0059] The mass fraction of the ammonia water in step A is 25%.
[0060] The particle size of the nano-silicon dioxide in step A is 50 nm.
[0061] The dropping rate in step B is controlled at 2 drops / s.
[0062] The mercaptosilane coupling agent in step B is γ-mercaptopropyltrimethoxysilane.
[0063] The long-chain olefin in step C is 1-tetradecene.
[0064] The wavelength of the ultraviolet light in step C is 365nm.
[0065] The polycarbonate is used in an amount of 75 parts by weight.
[0066] The amount of the polypropylene used is 35 parts by weight.
[0067] The amount of the modified filler is 10% of the total weight of the polycarbonate and the polypropylene.
[0068] A method for preparing a polycarbonate alloy, the method comprising the following steps:
[0069] Step a: mixing polycarbonate, polypropylene and modified filler in a mixer for 15 minutes to obtain a mixed material;
[0070] Step b: adding the mixed material into a twin-screw extruder for extrusion granulation, and the preparation is completed.
[0071] The operating parameters of the twin-screw extruder in step b are as follows: the processing temperature is controlled at 250° C., the screw speed is controlled at 700 rpm, and the feed rate is controlled at 25 kg / h.
[0072] Example 3
[0073] A polycarbonate alloy is prepared from polycarbonate, polypropylene and modified filler.
[0074] The polycarbonate was directly purchased from the market.
[0075] The polypropylene is directly purchased from the market.
[0076] The modified filler is prepared by the following steps:
[0077] Step A: 25 parts by weight of anhydrous ethanol and 18 parts by weight of aqueous ammonia are stirred at room temperature for 8 minutes, then 7 parts by weight of nano-silicon dioxide are added, stirred at 40° C. for 1.5 hours, filtered, the filtrate is removed, washed with anhydrous ethanol, and finally vacuum dried at 70° C. until constant weight is obtained to obtain hydroxylated nano-silicon dioxide;
[0078] Step B: adding 1.5 parts by weight of deionized water and the hydroxylated nano-silica to 65 parts by weight of anhydrous ethanol, and then dropping 5 parts by weight of a mercaptosilane coupling agent at 45° C. while stirring, and continuing to stir at a constant temperature for 22 hours after the dropwise addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 70° C. until constant weight, to obtain mercapto-modified nano-silica;
[0079] Step C: Add the mercapto-modified nano-silica and 0.8 parts by weight of benzoin dimethyl ether to 55 parts by weight of anhydrous ethanol, stir and mix at room temperature for 8 minutes, then add 3.5 parts by weight of long-chain olefins and 2.5 parts by weight of glycidyl methacrylate, stir at 28° C. for 1.5 hours under ultraviolet light, filter, remove the filtrate, wash with anhydrous ethanol, and finally vacuum dry at 70° C. until constant weight, and the preparation is completed.
[0080] The mass fraction of the ammonia water in step A is 23%.
[0081] The particle size of the nano-silicon dioxide in step A is 30 nm.
[0082] The dropping rate in step B is controlled at 1.5 drops / s.
[0083] The mercaptosilane coupling agent in step B is γ-mercaptopropyltrimethoxysilane.
[0084] The long-chain olefin in step C is 1-tetradecene.
[0085] The wavelength of the ultraviolet light in step C is 365nm.
[0086] The polycarbonate is used in an amount of 70 parts by weight.
[0087] The amount of polypropylene used is 33 parts by weight.
[0088] The modified filler is used in an amount of 9% of the total weight of the polycarbonate and the polypropylene.
[0089] A method for preparing a polycarbonate alloy, the method comprising the following steps:
[0090] Step a: mixing polycarbonate, polypropylene and modified filler in a mixer for 13 minutes to obtain a mixed material;
[0091] Step b: adding the mixed material into a twin-screw extruder for extrusion granulation, and the preparation is completed.
[0092] The operating parameters of the twin-screw extruder in step b are as follows: the processing temperature is controlled at 240° C., the screw speed is controlled at 600 rpm, and the feed rate is controlled at 23 kg / h.
[0093] Comparative Example 1
[0094] On the basis of Example 1, step A is omitted, the hydroxylated nano-silica in step B is replaced with nano-silica with a particle size of 20 nm, and the rest remain unchanged.
[0095] Comparative Example 2
[0096] On the basis of Example 1, 3 parts by weight of long-chain olefin in step C was changed to 2.5 parts by weight of long-chain olefin, and the rest remained unchanged.
[0097] Comparative Example 3
[0098] On the basis of Example 1, 3 parts by weight of long-chain olefin in step C was changed to 4.5 parts by weight of long-chain olefin, and the rest remained unchanged.
[0099] Comparative Example 4
[0100] On the basis of Example 1, 2 parts by weight of glycidyl methacrylate in step C was changed to 1.5 parts by weight of glycidyl methacrylate, and the rest remained unchanged.
[0101] Comparative Example 5
[0102] On the basis of Example 1, 2 parts by weight of glycidyl methacrylate in step C was changed to 3.5 parts by weight of glycidyl methacrylate, and the rest remained unchanged.
[0103] Comparative Example 6
[0104] On the basis of Example 1, the glycidyl methacrylate in step C was replaced with an equal weight portion of 1,2-epoxy-5-hexene, and the rest remained unchanged.
[0105] Comparative Example 7
[0106] On the basis of Example 1, the modified filler was changed to PP-g-GMA in equal parts by weight, and the rest remained unchanged.
[0107] Test Example 1
[0108] Mechanical properties test:
[0109] The polycarbonate alloys prepared in Examples 1-3 and Comparative Examples 1-7 were respectively added to an injection molding machine for injection molding to obtain corresponding test specimens, wherein the injection molding temperature was 250° C., the injection molding speed was 50 mm / s, and the injection molding pressure was 50 bar, and then the corresponding mechanical properties tests were performed, including:
[0110] Tensile strength (MPa) is tested according to standard GB / T 1040.1-2006. The size of the test specimens is 100mm*10mm*4mm, and the tensile speed is 50mm / min.
[0111] Izod notched impact strength (KJ / m 2 ), the test was carried out according to standard ISO 180-2000, the size of the test sample was 80mm*10mm*4mm, the pendulum energy was 5.5J, and the speed was 3.5m / s.
[0112] Table 1. Mechanical properties test results
[0113] Tensile Strength Izod notched impact strength Example 1 62.2 68.7 Example 2 63.9 70.6 Example 3 63.2 69.5 Comparative Example 1 52.8 55.1 Comparative Example 2 59.7 64.2 Comparative Example 3 59.2 63.9 Comparative Example 4 59.4 64.2 Comparative Example 5 58.8 63.3 Comparative Example 6 60.3 65.1 Comparative Example 7 47.8 49.9
[0114] Comparison between Example 1 and Comparative Examples 1-7 shows that:
[0115] The difference between Comparative Example 1 and Example 1 is that the nano-silicon dioxide is not subjected to hydroxylation treatment.
[0116] The difference between Comparative Example 2 and Example 1 is that the amount of long-chain olefin used is reduced.
[0117] The difference between Comparative Example 3 and Example 1 is that the amount of long-chain olefin used is increased.
[0118] The difference between Comparative Example 4 and Example 1 is that the amount of glycidyl methacrylate used is reduced.
[0119] The difference between Comparative Example 5 and Example 1 is that the amount of glycidyl methacrylate used is increased.
[0120] The difference between Comparative Example 6 and Example 1 is that the adjacent group of the epoxy group is not an ester group but a hydrocarbon group.
[0121] The difference between Comparative Example 7 and Example 1 is that no modified filler is added as a compatibilizer, but PP-g-GMA, which is currently commonly used, is used as a compatibilizer.
[0122] From the comparison between Example 1 and Comparative Examples 1-7 in Test Example 1, it can be seen that the components of the polycarbonate alloy prepared by the present invention are more compatible and have more excellent mechanical properties.
[0123] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A polycarbonate alloy, Features: The polycarbonate alloy is prepared from polycarbonate, polypropylene and modified filler; The modified filler is prepared by the following steps: Step A: 20-30 parts by weight of anhydrous ethanol and 15-20 parts by weight of aqueous ammonia are stirred at room temperature for 5-10 minutes, then 5-8 parts by weight of nano-silicon dioxide are added, stirred at 35-50° C. for 1-2 hours, filtered, the filtrate is removed, washed with anhydrous ethanol, and finally vacuum dried at 60-80° C. until constant weight is obtained to obtain hydroxylated nano-silicon dioxide; Step B: adding 1-2 parts by weight of deionized water and the hydroxylated nano-silica to 60-70 parts by weight of anhydrous ethanol, and then dropping 4-6 parts by weight of a mercaptosilane coupling agent at 40-50° C. while stirring, and continuing to stir at a constant temperature for 20-24 hours after the dropwise addition is completed, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 60-80° C. until constant weight, to obtain mercapto-modified nano-silica; Step C: adding the mercapto-modified nano-silica and 0.5-1 parts by weight of benzoin dimethyl ether to 50-60 parts by weight of anhydrous ethanol, stirring for 5-10 minutes at room temperature, then adding 3-4 parts by weight of long-chain olefin and 2-3 parts by weight of glycidyl methacrylate, stirring for 1-2 hours at 25-30° C. under ultraviolet light, filtering, removing the filtrate, washing with anhydrous ethanol, and finally vacuum drying at 60-80° C. until constant weight, and the preparation is completed; The mass fraction of the ammonia water in step A is 20-25%; The mercaptosilane coupling agent in step B is at least one of γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane; In step C, the long-chain olefin is at least one of dodecene and 1-tetradecene.
2. A polycarbonate alloy according to claim 1, Features: The dripping rate in step B is controlled at 1-2 drops / s.
3. A polycarbonate alloy according to claim 1, Features: The polycarbonate is used in an amount of 60-75 parts by weight.
4. A polycarbonate alloy according to claim 1, Features: The amount of polypropylene used is 30-35 parts by weight.
5. A polycarbonate alloy according to claim 1, Features: The amount of the modified filler is 8-10% of the total weight of the polycarbonate and the polypropylene.
6. A method for preparing a polycarbonate alloy as claimed in any one of claims 1 to 5, Features: The preparation method comprises the following steps: Step a: mixing polycarbonate, polypropylene and modified filler in a mixer for 10-15 minutes to obtain a mixed material; Step b: adding the mixed material into a twin-screw extruder for extrusion granulation, and the preparation is completed.