A modified asphalt specially used for high-performance porous graphite material and preparation method thereof
Through sedimentation treatment and catalytic modification technology, the problem of high asphalt impurity content in porous graphite materials is solved, the material performance and process efficiency are improved, the preparation of high-performance porous graphite materials is achieved, the process flow is simplified and energy consumption is reduced .
Patent Information
- Application Number
- CN202410881393.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-03
AI Technical Summary
The petroleum asphalt or coal tar pitch used in existing porous graphite materials has high impurity content, complex types of impurities, and unstable batch quality indicators. This results in long mixing times during the preparation process, unstable mesophase materials, and low finished product performance. The process flow is complex, energy consumption is high, and environmental friendliness is poor.
Using the methods of sedimentation treatment, primary catalytic modification and secondary catalytic modification, the softening point temperature, ash content and volatile matter content of the asphalt are controlled by combining the sedimentation treated asphalt with catalysts such as acidic alumina and vanadium oxide, and further The ineffective light components are discharged through the vacuum system to obtain modified asphalt specially designed for high-performance porous graphite materials.
It improves the compressive strength, dimensional stability, roasting qualification rate and high temperature stability of porous graphite materials, simplifies the process flow, reduces production energy consumption, improves product qualification rate and thermal conductivity, and improves the impurity content and quality of asphalt. Batch quality indicator stability.
Abstract
Description
Technical Field
[0001] The invention relates to the field of special graphite materials, in particular to a modified asphalt specially used for high-performance porous graphite materials and a preparation method thereof. Background Art
[0002] With the development of national strategic industries such as electronic semiconductors, green catalysis, and aerospace, porous graphite materials have become key materials in multiple application fields, playing an irreplaceable role in high-temperature gas transmission, loaded precious metal catalytic reactions, and spacecraft fuel mixing. Asphalt is an important raw material in the preparation process of porous graphite materials. In the existing porous graphite material production process, a kneading process is usually used to mix and preheat the raw materials such as aggregates and petroleum coke with good extraction ratios to a certain temperature, and then add them to the kneading device at the same time as petroleum asphalt or coal asphalt for kneading. In this process, asphalt acts as a binder, and through bonding, the aggregate particles are firmly bonded together to form a graphite structure with high strength and stability; at the same time, asphalt can also partially fill the gaps between aggregate particles, improve the density of the material, and thus improve the overall strength and thermal stability of the porous graphite material; and asphalt can also adjust the degree of graphitization in the preparation process of porous graphite materials, and stabilize the micro-tube structure of the material through the interaction between asphalt and aggregate particles under high temperature regulation, thereby achieving the purpose of adjusting the performance of porous graphite materials.
[0003] However, the petroleum asphalt or coal tar asphalt used in porous graphite on the market is not a special asphalt for porous graphite materials. It has many defects such as high impurity content, complex impurity types, unstable batch quality indicators, and poor content ratio of effective group components (such as toluene insolubles, quinoline insolubles, and β components). It will cause the mixing time required for the preparation of porous graphite materials to be long; and the intermediate phase material obtained by mixing is unstable, and cracking, low strength, and poor dimensional stability are prone to occur in the subsequent porous graphite molding process. The performance of the finished product and the qualified rate of the finished product need to be further improved. At the same time, it will also cause the residual carbon rate of the porous graphite material to be low, the degree of graphitization is not ideal, and it is easy to have defects such as unstable porosity control, low roasting qualified rate, and poor high-temperature stability. The process flow is long, the operation is cumbersome, the production efficiency is low, and the energy consumption is high.
[0004] In order to overcome the defects of existing asphalt, such as high impurity content, complex impurity types, unstable batch quality indicators and low content of effective group components, the existing technology usually adopts organic solvents to dissolve the asphalt, and then separates and removes impurities, heats and filters, centrifuges and other methods. However, it has the defects of complex operation, high processing energy consumption, high pollution, poor environmental friendliness, high equipment investment and high production risk.
[0005] Therefore, a modified asphalt specially used for high-performance porous graphite materials and a preparation method thereof are provided, which can overcome the aforementioned technical defects, and have important technical significance for the preparation of porous graphite materials. Summary of the invention
[0006] In order to solve the technical problems existing in the prior art, the present invention provides a modified asphalt specially used for high-performance porous graphite materials and a preparation method thereof, which can overcome the problem that the existing asphalt from various sources is not suitable for porous graphite materials, avoid the problems of cracking, low strength and poor dimensional stability that are prone to occur during the molding process of porous graphite materials, optimize the problems of unstable porosity control and low roasting qualification rate of conventional porous graphite, and further improve the strength, high-temperature stability and finished product qualification rate of isostatically pressed graphite materials.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing modified asphalt specially used for high-performance porous graphite material comprises the following steps: sedimentation treatment, primary catalytic modification, and secondary catalytic modification;
[0009] The sedimentation treatment method is to heat and melt the raw asphalt and then perform sedimentation treatment to obtain asphalt after sedimentation treatment;
[0010] The specific indicators of the raw asphalt are: softening point temperature of 70-100°C, ash content of 0.25-0.3wt%, volatile matter content of 58-61wt%, residual carbon content of 44-54wt%, toluene insoluble content of 15-25wt%, quinoline insoluble content of 8-14wt%, and β component content of 16-18wt%;
[0011] Preferably, the softening point temperature of the raw asphalt is 80-100°C.
[0012] The method of the primary catalytic modification is to introduce the asphalt after the sedimentation treatment into a reactor, stir and heat it to a temperature 30-70°C higher than the softening point of the asphalt, add the first catalyst, keep it warm and stir it to obtain a primary catalytic modified product;
[0013] The first catalyst is one of the following: acidic aluminum oxide, vanadium oxide, platinum oxide;
[0014] The secondary catalytic modification method comprises: adding a second catalyst to the primary catalytic modification product under the temperature conditions of the primary catalytic modification, controlling the vacuum degree in the reactor to be 0.07-0.085 MPa, carrying out the reaction at a heat preservation temperature, and cooling naturally to obtain a modified asphalt specially used for high-performance porous graphite materials;
[0015] The second catalyst is one of the following: dinitronaphthalene, thiourea, and ammonium nitrate.
[0016] Preferably, in the sedimentation treatment, the melting temperature is 170-200°C and the sedimentation treatment time is 40-48h.
[0017] Preferably, in the primary catalytic reforming, the heat preservation and stirring time after adding the first catalyst is 1-3 hours.
[0018] Preferably, in the primary catalytic modification, the added mass of the first catalyst is 0.1-2% of the total mass of the asphalt in the reactor; more preferably, the added mass of the first catalyst is 0.7-1% of the total mass of the asphalt in the reactor.
[0019] Preferably, in the secondary catalytic reforming, the insulation reaction time under the vacuum degree of 0.07-0.085 MPa is 1-3 h.
[0020] Preferably, in the secondary catalytic reforming, the added mass of the second catalyst is 2-5% of the total mass of the primary catalytic reforming product.
[0021] Furthermore, the sedimentation treatment method is to put the raw asphalt into an asphalt sedimentation tank with a conical bottom, start heating, and start stirring after the raw asphalt is melted during the heating process, and control the stirring rate to 30-80rpm; after the temperature rises to 170-200°C, keep warm and stir for 40-48 hours, open the discharge valve at the bottom of the asphalt sedimentation tank while it is hot, discharge the large particles of impurities settled in the conical area at the bottom of the asphalt sedimentation tank, and obtain the asphalt after sedimentation treatment.
[0022] A modified asphalt specially used for high-performance porous graphite material, prepared by the aforementioned preparation method;
[0023] In the modified asphalt specially used for high-performance porous graphite material, the content of toluene insoluble matter is greater than 30 wt %, the content of quinoline insoluble matter is less than 8 wt %, and the content of β component is greater than 25 wt %.
[0024] Furthermore, the modified asphalt specially used for high-performance porous graphite material has a softening point temperature of 150-180° C., an ash content of less than 0.3wt%, a volatile matter content of less than 58wt%, and a residual carbon content of 58-74wt%.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1) The method for preparing modified asphalt specially for high-performance porous graphite materials of the present invention aims at the defect that conventional asphalt can not be effectively applied to porous graphite materials, the characteristics of conventional asphalt, and the different roles played by effective group components (toluene insolubles, quinoline insolubles, β components) in conventional asphalt in the preparation of porous graphite materials. After the raw asphalt is subjected to a sedimentation treatment with specific operations and process parameters, the asphalt is subjected to a first catalytic modification using a first catalyst to adjust the content and ratio of effective group components in the asphalt and the molecular weight of the asphalt in the first catalytic modification; and then in the second catalytic modification, the second catalyst is used in combination with the first catalyst to synergistically catalyze polymerization to achieve the desired effect. Under certain operating and process parameter conditions, the content and content ratio of each effective group component in the asphalt are further controlled to a predetermined range, and the degree of asphalt polymerization and molecular weight level are controlled; and in the secondary catalytic modification process, combined with a reduced pressure environment, the ineffective light components that evaporate are discharged through a vacuum system to improve the controllability of the content and ratio of each effective group component in the asphalt. This can overcome the problem that asphalt from various existing sources is not suitable for porous graphite materials, avoid the problems of cracking, low strength, and poor dimensional stability that are prone to occur during the molding process of porous graphite materials, optimize the problems of unstable porosity control and low roasting qualification rate of conventional porous graphite, and further improve the strength, high temperature stability and finished product qualification rate of isostatic graphite materials.
[0027] 2) The preparation method of modified asphalt specially used for high-performance porous graphite material of the present invention can be applied to existing conventional commercially available raw material asphalt, and has strong raw material adaptability; after sedimentation treatment, primary catalytic modification, and secondary catalytic modification, the effective component content of the modified asphalt specially used for porous isostatic graphite material can be maintained within a predetermined range, effectively ensuring the application effect of the subsequent modified asphalt in high-performance porous graphite material, improving the stability of the intermediate phase material obtained by kneading in the porous graphite material, effectively avoiding the cracking problem of porous graphite during the molding process, and effectively improving the dimensional stability of porous graphite; at the same time, it can also improve the graphitization degree of porous graphite, improve product uniformity, and improve the high-temperature stability and thermal conductivity of porous graphite; and optimize the problem of unstable porosity of conventional porous graphite, improve the roasting qualification rate, shorten the process flow, improve production efficiency, and reduce production energy consumption.
[0028] 3) The modified asphalt specially used for high-performance porous graphite materials of the present invention has low impurity content and stable batch quality indicators. In view of the different roles played by effective group components (toluene insoluble matter, quinoline insoluble matter, β component) in conventional asphalt in the preparation of porous graphite materials, after sedimentation treatment, primary catalytic modification and secondary catalytic modification, the content and content ratio of each effective group component in the modified asphalt are effectively controlled to a predetermined range, and the residual carbon content of the modified asphalt is increased, thereby effectively improving the utilization rate of the modified asphalt in the preparation of high-performance porous graphite materials.
[0029] 4) The modified asphalt specially used for high-performance porous graphite material of the present invention has the following specific indicators: softening point temperature is 150-180°C, ash content is less than 0.3wt%, volatile matter content is less than 58wt%, residual carbon content is 58-74wt%, toluene insoluble matter (TI) content is greater than 30wt%, quinoline insoluble matter (QI) content is less than 8wt%, and β component content is greater than 25wt%. DETAILED DESCRIPTION
[0030] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0031] Example 1
[0032] This embodiment provides a method for preparing modified asphalt specially used for high-performance porous graphite materials, specifically:
[0033] 1. Sedimentation treatment
[0034] The raw asphalt is put into an asphalt settling tank with a conical bottom, and the temperature is started to rise. During the heating process, stirring is started after the raw asphalt is melted, and the stirring rate is controlled to be 60rpm. After the temperature rises to 180°C, the asphalt is stirred and settled for 48 hours under insulation, and the discharge valve at the bottom of the asphalt settling tank is opened while it is hot, and the large particles of impurities settled in the conical area at the bottom of the asphalt settling tank are discharged to obtain the asphalt after sedimentation treatment.
[0035] Among them, the specific indicators of the raw asphalt are as follows: softening point temperature is 82°C, ash content is 0.28wt%, volatile matter content is 60.5wt%, residual carbon content is 47wt%, toluene insoluble matter (TI) content is 16wt%, quinoline insoluble matter (QI) content is 13wt%, and β component content is 16wt%.
[0036] 2. Primary catalytic reforming
[0037] The asphalt obtained from the asphalt settling tank after sedimentation treatment was introduced into the reactor, stirred at 100 rpm and heated to 150°C (68°C higher than the asphalt softening point), the first catalyst was added, and the mixture was stirred for 2.5 hours to obtain a primary catalytic modified product.
[0038] Wherein, the first catalyst is acidic alumina.
[0039] The added mass of the first catalyst is 1% of the total mass of the asphalt in the reactor.
[0040] 3. Secondary catalytic reforming
[0041] Under the temperature condition of the first catalytic modification (i.e. 150°C), the second catalyst is added to the first catalytic modification product, the supporting vacuum system of the reactor is turned on, the vacuum degree in the reactor is controlled to be 0.08MPa, and the reaction is kept warm for 3 hours; at the same time, during the heat preservation reaction process, the ineffective light components are discharged by reduced pressure evaporation through the vacuum system; after the heat preservation reaction is completed, it is naturally cooled to obtain modified asphalt specially used for high-performance porous graphite materials.
[0042] Wherein, the second catalyst is ammonium nitrate.
[0043] The added mass of the second catalyst is 3% of the total mass of the first catalytic modified product.
[0044] This embodiment also provides a modified asphalt specially used for high-performance porous graphite material prepared by the aforementioned method.
[0045] After testing, the specific indicators of the modified asphalt specially used for high-performance porous graphite material of the present invention are: softening point temperature is 155°C, ash content is 0.22wt%, volatile matter content is 56.7wt%, residual carbon content is 64.1wt%, toluene insoluble matter (TI) content is 32.4wt%, quinoline insoluble matter (QI) content is 7.5wt%, and β component content is 26.8wt%.
[0046] Furthermore, the modified asphalt specially used for high-performance porous graphite materials of the present invention is used in the preparation of porous graphite materials. Compared with directly using the aforementioned raw asphalt, under the same addition amount conditions, the compressive strength of the prepared porous graphite material is increased by 12.5%, and the stability of the intermediate phase material obtained by kneading in the porous graphite material can be improved, and the cracking problem of isostatic graphite during the molding process can be effectively avoided. The qualified rate of porous graphite products is increased by more than 9%; at the same time, the modified asphalt specially used for high-performance porous graphite materials of the present invention is used in the preparation of porous graphite materials, which can optimize the unstable control of the porosity of conventional porous graphite, improve the roasting qualified rate, greatly shorten the process flow, improve production efficiency, reduce production energy consumption, and improve the density uniformity of porous graphite materials; and it can also further improve the high temperature stability and thermal conductivity of porous graphite.
[0047] Example 2
[0048] This embodiment provides a method for preparing modified asphalt specially used for high-performance porous graphite materials, specifically:
[0049] 1. Sedimentation treatment
[0050] The raw asphalt is put into an asphalt settling tank with a conical bottom, and the temperature is started to rise. During the heating process, stirring is started after the raw asphalt is melted, and the stirring rate is controlled to be 70rpm. After the temperature rises to 190°C, the asphalt is kept stirred and settled for 46 hours, and the discharge valve at the bottom of the asphalt settling tank is opened while it is hot, and the large particles of impurities settled in the conical area at the bottom of the asphalt settling tank are discharged to obtain the asphalt after sedimentation treatment.
[0051] Among them, the specific indicators of the raw asphalt are as follows: softening point temperature is 99°C, ash content is 0.28wt%, volatile matter content is 60.5wt%, residual carbon content is 47wt%, toluene insoluble matter (TI) content is 16wt%, quinoline insoluble matter (QI) content is 13wt%, and β component content is 16wt%.
[0052] 2. Primary catalytic reforming
[0053] The asphalt obtained from the asphalt settling tank after sedimentation treatment was introduced into the reactor, stirred at 90 rpm and heated to 155°C (56°C higher than the asphalt softening point), the first catalyst was added, and the mixture was stirred for 2 hours to obtain a primary catalytic modified product.
[0054] Wherein, the first catalyst is vanadium oxide.
[0055] The added mass of the first catalyst is 0.7% of the total mass of asphalt in the reactor.
[0056] 3. Secondary catalytic reforming
[0057] Under the temperature condition of the first catalytic modification (i.e. 155°C), the second catalyst is added to the first catalytic modification product, the vacuum system of the reactor is turned on, the vacuum degree in the reactor is controlled to be 0.085MPa, and the reaction is kept warm for 2 hours; at the same time, during the heat preservation reaction, the ineffective light components evaporated under reduced pressure are discharged through the vacuum system; after the heat preservation reaction is completed, it is cooled naturally to obtain modified asphalt specially used for high-performance porous graphite materials.
[0058] Wherein, the second catalyst is dinitronaphthalene.
[0059] The added mass of the second catalyst is 4.5% of the total mass of the first catalytic modified product.
[0060] This embodiment also provides a modified asphalt specially used for high-performance porous graphite material prepared by the aforementioned method.
[0061] After testing, the specific indicators of the modified asphalt specially used for high-performance porous graphite material of the present invention are: softening point temperature is 160°C, ash content is 0.23wt%, volatile matter content is 56.4wt%, residual carbon content is 63.9wt%, toluene insoluble matter (TI) content is 32.3wt%, quinoline insoluble matter (QI) content is 7.4wt%, and β component content is 27wt%.
[0062] Furthermore, the modified asphalt specially used for high-performance porous graphite materials of the present invention is used in the preparation of porous graphite materials. Compared with directly using the aforementioned raw asphalt, under the same addition conditions, the compressive strength of the prepared porous graphite material is increased by 12.1%, and the stability of the intermediate phase material obtained by kneading in the isostatically pressed graphite material can be improved, and the cracking problem of porous graphite during the molding process can be effectively avoided. The qualified rate of porous graphite products is increased by more than 9%; at the same time, the modified asphalt specially used for high-performance porous graphite materials of the present invention is used in the preparation of porous graphite materials, which can optimize the instability of the porosity control of porous graphite, improve the roasting qualified rate, greatly shorten the process flow, improve production efficiency, reduce production energy consumption, and improve the density uniformity of porous graphite materials; and it can also further improve the high temperature stability and thermal conductivity of porous graphite.
[0063] Example 3
[0064] This embodiment provides a method for preparing modified asphalt specially used for high-performance porous graphite materials, specifically:
[0065] 1. Sedimentation treatment
[0066] The raw asphalt is put into an asphalt settling tank with a conical bottom, and the temperature is started to rise. During the heating process, stirring is started after the raw asphalt is melted, and the stirring rate is controlled to be 40rpm. After the temperature rises to 200℃, the asphalt is stirred and settled for 42 hours under insulation, and the discharge valve at the bottom of the asphalt settling tank is opened while it is hot, and the large particles of impurities settled in the conical area at the bottom of the asphalt settling tank are discharged to obtain the asphalt after sedimentation treatment.
[0067] Among them, the specific indicators of the raw asphalt are as follows: softening point temperature is 89°C, ash content is 0.28wt%, volatile matter content is 60.5wt%, residual carbon content is 47wt%, toluene insoluble matter (TI) content is 16wt%, quinoline insoluble matter (QI) content is 13wt%, and β component content is 16wt%.
[0068] 2. Primary catalytic reforming
[0069] The asphalt obtained from the asphalt settling tank after sedimentation treatment was introduced into the reactor, stirred at 80 rpm and heated to 140°C (51°C higher than the softening point of asphalt), the first catalyst was added, and the mixture was stirred for 3 hours to obtain a primary catalytic modified product.
[0070] Wherein, the first catalyst is platinum oxide.
[0071] The added mass of the first catalyst is 0.9% of the total mass of asphalt in the reactor.
[0072] 3. Secondary catalytic reforming
[0073] Under the temperature condition of the first catalytic modification (i.e. 140°C), the second catalyst is added to the first catalytic modification product, the supporting vacuum system of the reactor is turned on, the vacuum degree in the reactor is controlled to be 0.08MPa, and the reaction is kept warm for 3 hours; at the same time, during the heat preservation reaction process, the ineffective light components are discharged by reduced pressure evaporation through the vacuum system; after the heat preservation reaction is completed, it is naturally cooled to obtain modified asphalt specially used for high-performance porous graphite materials.
[0074] Wherein, the second catalyst is thiourea.
[0075] The added mass of the second catalyst is 2.5% of the total mass of the first catalytic modified product.
[0076] This embodiment also provides a modified asphalt specially used for high-performance porous graphite material prepared by the aforementioned method.
[0077] After testing, the specific indicators of the modified asphalt specially used for high-performance porous graphite material of the present invention are: softening point temperature is 165°C, ash content is 0.24wt%, volatile matter content is 56wt%, residual carbon content is 64.3wt%, toluene insoluble matter (TI) content is 33.2wt%, quinoline insoluble matter (QI) content is 7.3wt%, and β component content is 25.8wt%.
[0078] Furthermore, the modified asphalt specially used for high-performance porous graphite materials of the present invention is used in the preparation of porous graphite materials. Compared with directly using the aforementioned raw asphalt, under the same addition amount conditions, the compressive strength of the prepared porous graphite material is increased by 12%, and the stability of the intermediate phase material obtained by kneading in the porous graphite material can be improved, and the cracking problem of porous graphite during the molding process can be effectively avoided. The qualified rate of porous graphite products is increased by more than 11%; at the same time, the use of the modified asphalt specially used for high-performance porous graphite materials of the present invention in the preparation of porous graphite materials can simplify the multiple impregnation and roasting processes in the traditional process, greatly shorten the process flow, improve production efficiency, reduce production energy consumption, and improve the density uniformity of the porous graphite material; and it can also further improve the high temperature stability and thermal conductivity of the porous graphite.
[0079] Unless otherwise specified, all percentages used in the present invention are by mass.
[0080] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing modified asphalt specially used for high-performance porous graphite material, characterized in that: The method comprises the following steps: sedimentation treatment, primary catalytic reforming, and secondary catalytic reforming; The sedimentation treatment method is to heat and melt the raw asphalt and then perform sedimentation treatment to obtain asphalt after sedimentation treatment; The specific indicators of the raw asphalt are: softening point temperature of 70-100°C, ash content of 0.25-0.3wt%, volatile matter content of 58-61wt%, residual carbon content of 44-54wt%, toluene insoluble content of 15-25wt%, quinoline insoluble content of 8-14wt%, and β component content of 16-18wt%; The method of the primary catalytic modification is to introduce the asphalt after the sedimentation treatment into a reactor, stir and heat it to a temperature 30-70°C higher than the softening point of the asphalt, add the first catalyst, keep it warm and stir it to obtain a primary catalytic modified product; The first catalyst is one of the following: acidic aluminum oxide, vanadium oxide, platinum oxide; The added mass of the first catalyst is 0.1-2% of the total mass of the asphalt in the reactor; The secondary catalytic modification method comprises: adding a second catalyst to the primary catalytic modification product under the temperature conditions of the primary catalytic modification, controlling the vacuum degree in the reactor to be 0.07-0.085 MPa, carrying out the reaction at a heat preservation temperature, and cooling naturally to obtain a modified asphalt specially used for high-performance porous graphite materials; The second catalyst is one of the following: dinitronaphthalene, thiourea, ammonium nitrate; The added mass of the second catalyst is 2-5% of the total mass of the first catalytic modified product.
2. The method for preparing modified asphalt specially made for high-performance porous graphite material according to claim 1, characterized in that: In the sedimentation treatment, the melting temperature is 170-200° C. and the sedimentation treatment time is 40-48 hours.
3. The method for preparing modified asphalt specially used for high-performance porous graphite material according to claim 1, characterized in that: In the primary catalytic reforming, the heat preservation and stirring time after adding the first catalyst is 1-3 hours.
4. The method for preparing modified asphalt specially used for high-performance porous graphite material according to claim 1, characterized in that: In the secondary catalytic reforming, the heat preservation reaction time is 1-3h under the condition of vacuum degree of 0.07-0.085MPa.
5. The method for preparing modified asphalt specially used for high-performance porous graphite material according to claim 1, characterized in that: The sedimentation treatment method is as follows: the raw asphalt is put into an asphalt sedimentation tank with a conical bottom, the temperature is started to be increased, stirring is started after the raw asphalt is melted during the heating process, and the stirring rate is controlled to be 30-80rpm; after the temperature is heated to 170-200°C, the mixture is kept warm and stirred for 40-48h, the discharge valve at the bottom of the asphalt sedimentation tank is opened while it is hot, and the large particle impurities settled in the conical area at the bottom of the asphalt sedimentation tank are discharged to obtain the asphalt after sedimentation treatment.
6. A modified asphalt specially made for high-performance porous graphite material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 5; In the modified asphalt specially used for high-performance porous graphite material, the content of toluene insoluble matter is greater than 30 wt %, the content of quinoline insoluble matter is less than 8 wt %, and the content of β component is greater than 25 wt %.
7. The modified asphalt specially used for high-performance porous graphite material according to claim 6, characterized in that: The modified asphalt specially used for high-performance porous graphite material has a softening point temperature of 150-180° C., an ash content of less than 0.3wt%, a volatile matter content of less than 58wt%, and a residual carbon content of 58-74wt%.