Flame retardant adhesive composition, flame retardant tape and preparation method

By using a combination of epoxy resin, acrylic copolymer, ammonium polyphosphate and modified expanded graphite in the flame retardant tape, the problems of high volatility, poor heat resistance and dripping after combustion of the flame retardant tape are solved. It achieves high-efficiency halogen-free flame retardant effect and excellent bonding performance.

CN118421246BActive Publication Date: 2024-12-03HEYUAN KUNTENG ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410441964.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-12-03
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

The existing flame retardant tapes have problems such as high organic volatility, poor heat resistance, unsatisfactory compatibility and drippings after combustion.

Method used

Using epoxy resin and acrylic copolymer as matrix materials, combined with ammonium polyphosphate, carboxymethyl cellulose calcium and modified expanded graphite, improve the adhesive performance and flame retardant properties through curing reaction and compounding technology, and expand the graphite Under the control of particle size, the production of smoke and drips is inhibited.

Benefits of technology

It achieves high-efficiency, halogen-free flame retardant effect, no dripping during combustion, no obvious smoke, excellent bonding performance, and reaches the flame retardant level of UL94 VTM-0.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004789476300000051
    Figure BDA0004789476300000051
  • Figure BDA0004789476300000081
    Figure BDA0004789476300000081
  • Figure BDA0004789476300000091
    Figure BDA0004789476300000091
Patent Text Reader

Abstract

The present application belongs to the technical field of flame retardant tapes, and the present application discloses a flame retardant adhesive composition, a flame retardant tape, and a preparation method. The raw materials of the flame retardant adhesive composition in the present application include epoxy resin, acrylic copolymer, ammonium polyphosphate, carboxymethyl cellulose calcium, expanded graphite, curing agent, diluent, and defoaming agent. The flame retardant tape in the present application achieves the UL94 VTM‑0 flame retardant rating of the tape, and achieves post-combustion expansion and smoke suppression through the design combination of compounded flame retardants, and achieves no dripping and no obvious smoke generation during the combustion process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of flame retardant tapes, and in particular to a flame retardant adhesive composition, a flame retardant tape and a preparation method thereof. Background Art

[0002] Flame retardant tape is a flame retardant tape, which is widely used in the fixing and wrapping of various electronic components such as plasma and LCD TVs, monitors, and automotive wiring harnesses. At present, most of the widely used flame retardant tapes use one or more halogen-containing flame retardants, and the use of halogen-containing flame retardants has environmental and safety issues.

[0003] Epoxy resin adhesives have excellent bonding properties, mechanical strength, moisture and heat resistance, impact resistance and corrosion resistance, and are widely used in the electronic and electrical industry. At the same time, epoxy adhesives can be cured at room temperature or by heating, which can meet the different application needs of customers. However, epoxy resin has a low oxygen index (about 19.8), which is a flammable material. In addition, epoxy resin is easy to drip, and it continues to spontaneously combust after being removed from the fire, which is easy to cause a fire. Therefore, it is necessary to modify the epoxy adhesive to be flame retardant. After adding halogen-free flame retardants and flame retardant synergists to epoxy resin, the material combustion level is increased from UL-94V-2 to V-0 level, which effectively reduces the flammability of the material; adding hyperbranched macromolecular flame retardant carbonizing agents to the adhesive, due to the presence of more carbon atoms in the molecular structure, chemical reactions occur during combustion to form a porous expanded carbon layer, which is not easy to burn, and can play a role in heat insulation, smoke suppression, and dripping resistance, thereby also achieving the purpose of flame retardancy. However, the halogen-free flame retardants currently on the market do not show excellent flame retardant properties. The flame retardant effect is poor when the amount added is small, and there are problems such as poor compatibility between the flame retardant and the polymer adhesive and affecting product quality when added in large quantities, and the performance is not guaranteed. Commonly used flame retardant tapes still have problems such as high volatility of organic matter after combustion, poor heat resistance, and unsatisfactory compatibility, and there are also disadvantages such as dripping when burning. Summary of the invention

[0004] In order to solve at least one of the above technical problems, a flame retardant tape with good flame retardant effect, strong adhesive performance, no dripping during combustion and no obvious smoke generation is developed. The present application provides a flame retardant adhesive composition, a flame retardant tape and a preparation method.

[0005] In a first aspect, the present application provides a flame retardant adhesive composition, comprising the following raw materials in parts by weight: 80-110 parts of epoxy resin, 40-75 parts of acrylic copolymer, 7-13 parts of ammonium polyphosphate, 4-6 parts of carboxymethyl cellulose calcium, 2-4.5 parts of expanded graphite, 6-11 parts of curing agent, 8-16 parts of diluent, and 2-4 parts of defoaming agent.

[0006] By adopting the above technical scheme, epoxy resin and acrylic copolymer are used as the matrix materials of the flame retardant adhesive composition, and the acrylic polymer and the epoxy resin will react through the side chain carboxyl of the acrylic polymer and the epoxy group of the epoxy resin to cure, thereby further improving the adhesive performance and shear strength of the adhesive. Calcium carboxymethyl cellulose has good adhesion and adhesiveness, and can be used as a thickener in the adhesive to improve the dispersibility of powder materials such as expanded graphite in the epoxy resin; on the other hand, calcium carboxymethyl cellulose has good self-expansion under heating conditions, and plays the role of carbon source and gas source when compounded with ammonium polyphosphate; the ammonium polyphosphate, calcium carboxymethyl cellulose and amine curing agent in the present application are respectively used as the acid source, carbon source and gas source in the IFR flame retardant, and the flame retardant performance of the flame retardant adhesive composition is improved under the premise of maintaining strong adhesive performance, and the expanded graphite modified by ferrocene ketone is also added, so as to suppress the generation of smoke and dripping during the burning process of the tape.

[0007] Preferably, the flame retardant adhesive composition comprises the following raw materials in parts by weight: 100 parts of epoxy resin, 55 parts of acrylic polymer, 12 parts of ammonium polyphosphate, 5.5 parts of calcium carboxymethyl cellulose, 4 parts of expanded graphite, 9 parts of curing agent, 10 parts of diluent, and 2.5 parts of defoaming agent.

[0008] By adopting the above technical scheme, when the amount of flame retardant or flame retardant synergist (expanded graphite) is too much, it will seriously affect the bonding performance of the flame retardant adhesive composition; the applicant repeatedly adjusts the ratio of each component to increase the amount of flame retardant without reducing the bonding performance of the flame retardant adhesive composition, thereby further improving its smoke suppression and anti-drip performance.

[0009] Optionally, the particle size of the expanded graphite is 0.5-5 um.

[0010] By adopting the above technical solution, if the particle size of the expanded graphite is too small, it will seriously affect its expansion and foaming during the combustion process, resulting in the porous foam carbon layer formed at high temperature having low strength and easy to break, thereby failing to achieve the effect of smoke suppression and drip suppression; if the particle size of the expanded graphite is too large, it will affect the bonding properties of the flame retardant adhesive composition; therefore, it is necessary to control the particle size of the expanded graphite within a suitable range.

[0011] Optionally, the acrylic copolymer includes one or more of methyl acrylate-acrylic acid copolymer, methyl methacrylate-acrylic acid copolymer, ethyl acrylate-acrylic acid copolymer, hydroxyethyl acrylate-acrylic acid copolymer, hydroxypropyl acrylate-acrylic acid copolymer, n-butyl acrylate-acrylic acid copolymer, isooctyl acrylate-acrylic acid copolymer and glycidyl methacrylate-acrylic acid copolymer.

[0012] Preferably, the acrylic copolymer comprises hydroxypropyl acrylate-acrylic acid copolymer and isooctyl acrylate-acrylic acid copolymer in a weight ratio of 2-4:5-8.

[0013] Preferably, the preparation method of the hydroxypropyl acrylate-acrylic acid copolymer is as follows: hydroxypropyl acrylate and acrylic acid in a molar ratio of 4:1 are added to a solvent toluene, and under the protection of an inert gas, at 60-80° C., an initiator azobisisobutyronitrile is added, and the reaction is kept warm for 6 hours to obtain the hydroxypropyl acrylate-acrylic acid copolymer; the amount of the initiator used is 1-2wt% of the total amount of the polymerization monomers.

[0014] Preferably, the preparation method of the isooctyl acrylate-acrylic acid copolymer is as follows: isooctyl acrylate and acrylic acid in a molar ratio of 4:1 are added to a solvent toluene, and under the protection of an inert gas, at 60-80° C., an initiator azobisisobutyronitrile is added, and the reaction is kept warm for 6 hours to obtain the isooctyl acrylate-acrylic acid copolymer; the amount of the initiator used is 1-2wt% of the total amount of the polymerization monomers.

[0015] By adopting the above technical scheme, the flame retardant adhesive composition of the present application uses acrylic polymer as the main adhesive substrate, and the acrylic copolymer in the present application can be obtained by copolymerization using an acrylate monomer as the first monomer and acrylic acid as the second monomer. Among them, when the acrylic acid repeating unit is more than 15%, the flame retardant adhesive composition obtained has higher adhesive properties. In the present application, the acrylate monomer used as the first monomer for forming the acrylic copolymer is preferably hydroxypropyl acrylate and isooctyl acrylate. The acrylic copolymer formed by copolymerizing the former as the first monomer and acrylic acid as the second monomer has better water resistance and weather resistance, which is beneficial to prolonging the service life of the flame retardant tape.

[0016] Optionally, the curing agent includes one or more of ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, polyetheramine, m-phenylenediamine, diphenylmethanediamine, isophoronediamine and polyamide.

[0017] Optionally, the expanded graphite is modified expanded graphite.

[0018] Optionally, the method for preparing the modified expanded graphite comprises the following steps:

[0019] (1) adding acetylferrocene, formaldehyde, sodium hydroxide and potassium carbonate into a container, grinding at 15-30° C. for 5-10 min, washing with water, and drying to obtain ferrocene ketone, which is then set aside;

[0020] (2) 98 wt% concentrated sulfuric acid, hydrogen peroxide and graphite are mixed, reacted for 80-120 min, dried, heat treated, added to an acetone solution of ferrocenyl ketone, ultrasonically dispersed, filtered and dried to obtain modified expanded graphite.

[0021] By adopting the above technical scheme, ferrocene has a smoke suppression effect on epoxy resin, but since it also has a combustion-supporting effect, it will reduce the flame retardant efficiency of the phosphorus-based flame retardant; in the present application, ferrocene ketone is used to modify the expanded graphite, and the porous foam carbon layer produced after the expanded graphite is heated will not be significantly affected by the combustion-supporting effect of ferrocene, but it can greatly reduce the smoke flying out of the porous foam carbon layer, and can also reduce the generation of dripping materials.

[0022] In a second aspect, the present application provides a method for preparing the flame retardant adhesive composition, comprising the following steps:

[0023] Mix the epoxy resin, diluent and defoamer, heat to 50-75°C, stir for 0.5-1h, heat to 85-95°C, add expanded graphite and acrylic copolymer, stir for 1-2h; cool to 50-75°C, add the remaining raw materials, stir for 1-2h to obtain a flame retardant adhesive composition.

[0024] In a third aspect, the present application provides a flame retardant tape, comprising a substrate and a flame retardant adhesive composition coated on one side of the substrate, the substrate being selected from one of a polypropylene film, a polyvinyl chloride film, a polyimide film and a polyester film, and the flame retardant adhesive composition being the flame retardant adhesive composition described in any one of claims 1 to 7.

[0025] In a fourth aspect, the present application provides a method for preparing a flame retardant tape made from the flame retardant adhesive composition, comprising the following steps:

[0026] The flame retardant adhesive composition is coated on one side of a substrate, dried at a temperature range of 70-140° C., and rolled up after natural cooling to obtain a flame retardant tape.

[0027] In summary, the present invention includes at least one of the following beneficial technical effects:

[0028] 1. The present application provides a highly efficient halogen-free flame-retardant flame-retardant adhesive composition and a flame-retardant tape, which have the characteristics of good flame retardant effect, anti-dripping, low smoke emission, and excellent bonding performance.

[0029] 2. The flame retardant tape in this application achieves the UL94 VTM-0 flame retardant rating of the tape, and achieves post-combustion expansion and smoke suppression through the design combination of compound flame retardants, so that there is no dripping and no obvious smoke generation during the combustion process. DETAILED DESCRIPTION

[0030] The present application is further described in detail below with reference to the embodiments.

[0031] The present application designs a flame retardant adhesive composition, which includes the following raw materials in parts by weight: 80-110 parts of epoxy resin, 40-75 parts of acrylic copolymer, 7-13 parts of ammonium polyphosphate, 4-6 parts of carboxymethyl cellulose calcium, 2-4.5 parts of expanded graphite, 6-11 parts of curing agent, 8-16 parts of diluent, and 2-4 parts of defoaming agent.

[0032] The expanded graphite is modified expanded graphite, and the preparation method of the modified expanded graphite comprises the following steps:

[0033] (1) adding acetylferrocene, formaldehyde, sodium hydroxide and potassium carbonate into a container, grinding at 15-30° C. for 5-10 min, washing with water, and drying to obtain ferrocene ketone for later use;

[0034] (2) 98 wt% concentrated sulfuric acid, hydrogen peroxide and graphite are mixed, reacted for 80-120 min, dried, heat treated, added to an acetone solution of ferrocenyl ketone, ultrasonically dispersed, filtered and dried to obtain modified expanded graphite.

[0035] The flame retardant adhesive composition of the present application is prepared by the following method, comprising the following steps:

[0036] Mix the epoxy resin, diluent and defoamer, heat to 50-75°C, stir for 0.5-1h, heat to 85-95°C, add expanded graphite and acrylic copolymer, stir for 1-2h; cool to 50-75°C, add the remaining raw materials, stir for 1-2h to obtain a flame retardant adhesive composition.

[0037] The present application designs a flame retardant tape made from the above flame retardant adhesive composition, wherein the flame retardant tape consists of a substrate and a flame retardant adhesive composition coated on one side of the substrate, wherein the substrate is selected from one of polypropylene film, polyvinyl chloride film, polyimide film and polyester film.

[0038] The flame retardant tape prepared from the flame retardant adhesive composition of the present application is prepared by the following method, comprising the following steps:

[0039] The flame retardant adhesive composition is coated on one side of a substrate, dried at a temperature range of 70-140° C. for 2-10 minutes, and rolled up after natural cooling to obtain a flame retardant tape.

[0040] The technical problem solved by this application is that the flame retardant tapes currently on the market have the problems of high volatility of organic matter after combustion, poor heat resistance, unsatisfactory compatibility, and the generation of drips during combustion. This application uses epoxy resin and acrylic copolymer as the base material of the flame retardant adhesive composition, and ammonium polyphosphate, calcium carboxymethyl cellulose and amine curing agent as the acid source, carbon source and gas source in the IFR flame retardant respectively, to improve the flame retardant performance of the flame retardant adhesive composition while maintaining strong bonding performance, and also adds expanded graphite modified with ferrocenium ketone, so as to suppress the generation of smoke and drips during the burning process of the tape.

[0041] The raw materials used in the examples of this application are all commercially available from the following sources:

[0042] Bisphenol A epoxy resin, Guangdong Wengjiang Chemical Reagent Co., Ltd.;

[0043] Hexamethylenediamine, Guangdong Wengjiang Chemical Reagent Co., Ltd.;

[0044] Polyethylene glycol diglycidyl ether, Zhongshan Dixin Chemical Co., Ltd.;

[0045] BYK066N, BYK Additives (Shanghai) Co., Ltd.;

[0046] Acetylferrocene, Sigma-Aldrich (Shanghai) Trading Co., Ltd.;

[0047] Calcium carboxymethyl cellulose, Sigma-Aldrich (Shanghai) Trading Co., Ltd.

[0048] Examples 1-5

[0049] Examples 1-5 are flame retardant adhesive compositions prepared with different raw material ratios, the difference being that the amounts of each component are different. The specific raw material ratios and amounts are shown in Table 1. (The units of the amounts of each component in Table 1 are parts by weight)

[0050] Table 1

[0051]

[0052] The acrylic copolymers used in Examples 1-5 are hydroxypropyl acrylate-acrylic acid copolymer and isooctyl acrylate-acrylic acid copolymer in a weight ratio of 2.5:6.

[0053] The preparation method of hydroxypropyl acrylate-acrylic acid copolymer is as follows: hydroxypropyl acrylate and acrylic acid in a molar ratio of 4:1 are added to a solvent toluene, and under the protection of an inert gas, an initiator azobisisobutyronitrile is added at 80° C., and the reaction is kept warm for 6 hours to obtain a hydroxypropyl acrylate-acrylic acid copolymer; the amount of the initiator used is 1.5wt% of the total amount of the polymerization monomers.

[0054] The preparation method of isooctyl acrylate-acrylic acid copolymer is as follows: isooctyl acrylate and acrylic acid in a molar ratio of 4:1 are added to a solvent toluene, and under the protection of an inert gas, an initiator azobisisobutyronitrile is added at 80° C., and the reaction is kept warm for 6 hours to obtain the isooctyl acrylate-acrylic acid copolymer; the amount of the initiator used is 1.5wt% of the total amount of the polymerization monomers.

[0055] The epoxy resins used in Examples 1-5 are all bisphenol A epoxy resins.

[0056] The curing agent used in Examples 1-5 is hexamethylenediamine.

[0057] The diluent used in Examples 1-5 is polyethylene glycol diglycidyl ether.

[0058] The defoamer used in Examples 1-5 is BYK066N.

[0059] The average particle size of the expanded graphite used in Examples 1-5 is about 1.5 um.

[0060] The preparation process of the expanded graphite used in Examples 1-5 is as follows:

[0061] 98wt% concentrated sulfuric acid, hydrogen peroxide and graphite are mixed, reacted for 100 minutes, dried, heat treated at 900°C for 20 seconds, added to an acetone solution, ultrasonically dispersed for 8 hours, filtered, dried, and expanded graphite is obtained, and expanded graphite of corresponding particle size is obtained by grinding; wherein, the weight ratio of 98wt% concentrated sulfuric acid, hydrogen peroxide and graphite is 10:3:16.

[0062] The preparation process of the flame retardant adhesive composition in Examples 1-5 is as follows:

[0063] The epoxy resin, diluent and defoamer were mixed, heated to 70°C, stirred for 1 hour, heated to 90°C, expanded graphite and acrylic copolymer were added, and stirred for 2 hours; cooled to 70°C, the remaining raw materials were added, stirred for 2 hours, and cooled naturally to obtain a flame retardant adhesive composition.

[0064] Embodiment 6-9

[0065] Example 6 is based on Example 2, except that the acrylic copolymer used in Example 6 is a hydroxypropyl acrylate-acrylic acid copolymer and an isooctyl acrylate-acrylic acid copolymer in a weight ratio of 2:8.

[0066] Example 7 is based on Example 2, except that the acrylic copolymer used in Example 7 is a hydroxypropyl acrylate-acrylic acid copolymer and an isooctyl acrylate-acrylic acid copolymer in a weight ratio of 4:5.

[0067] Example 8 is based on Example 2, except that the acrylic copolymer used in Example 8 is a hydroxypropyl acrylate-acrylic acid copolymer and a n-butyl acrylate-acrylic acid copolymer in a weight ratio of 2.5:6.

[0068] The preparation method of n-butyl acrylate-acrylic acid copolymer is as follows: n-butyl acrylate and acrylic acid in a molar ratio of 4:1 are added to a solvent toluene, and under the protection of an inert gas, an initiator azobisisobutyronitrile is added at 80° C., and the reaction is kept warm for 6 hours to obtain n-butyl acrylate-acrylic acid copolymer; the amount of the initiator used is 1.5wt% of the total amount of the polymerization monomers.

[0069] Example 9 is based on Example 2, except that the acrylic copolymer used in Example 9 is an ethyl acrylate-acrylic acid copolymer and an isooctyl acrylate-acrylic acid copolymer in a weight ratio of 2.5:6.

[0070] The preparation method of ethyl acrylate-acrylic acid copolymer is as follows: ethyl acrylate and acrylic acid in a molar ratio of 4:1 are added to a solvent toluene, and under the protection of an inert gas, an initiator azobisisobutyronitrile is added at 80° C., and the reaction is kept warm for 6 hours to obtain the ethyl acrylate-acrylic acid copolymer; the amount of the initiator used is 1.5wt% of the total amount of the polymerization monomers.

[0071] Examples 10-12

[0072] Example 10 is based on Example 2, except that the average particle size of the expanded graphite used in Example 10 is about 0.5 um.

[0073] Example 11 is based on Example 2, except that the average particle size of the expanded graphite used in Example 11 is about 5 um.

[0074] Example 12 is based on Example 2, except that the average particle size of the expanded graphite used in Example 12 is about 0.05 um.

[0075] Embodiment 13

[0076] Example 13 is based on Example 2, except that the expanded graphite used in Example 13 is modified expanded graphite; the average particle size of the modified expanded graphite is about 1.5 um.

[0077] The preparation method of the modified expanded graphite is:

[0078] (1) Add acetylferrocene, formaldehyde, sodium hydroxide and potassium carbonate into a container, grind at room temperature for 10 minutes, wash with water until neutral, and dry to obtain ferrocenyl ketone for later use; wherein the weight ratio of acetylferrocene, formaldehyde, sodium hydroxide and potassium carbonate is 5:1.5:0.4:0.4.

[0079] (2) 98 wt% concentrated sulfuric acid, hydrogen peroxide and graphite are mixed, reacted for 100 min, dried, heat treated at 900°C for 20 s, cooled to room temperature, added to 10 wt% ferrocenyl ketone in acetone, ultrasonically dispersed for 8 h, filtered and dried to obtain modified expanded graphite; wherein the weight ratio of 98 wt% concentrated sulfuric acid, hydrogen peroxide, graphite and ferrocenyl ketone is 10:3:16:5.

[0080] Comparative Example 1

[0081] Comparative Example 1 is based on Example 2, except that no expanded graphite is added in Comparative Example 1.

[0082] Comparative Example 2

[0083] Comparative Example 2 is based on Example 2, except that the amount of expanded graphite in Comparative Example 2 is increased to 8 parts by weight.

[0084] Comparative Example 3

[0085] Comparative Example 3 is based on Example 2, except that in Comparative Example 3, calcium carboxymethyl cellulose is replaced by another carbon source, pentaerythritol.

[0086] Application Examples 1-13 and Comparative Application Examples 1-3

[0087] Application Examples 1-13 and Application Comparative Examples 1-3 are flame-retardant tapes made from the flame-retardant adhesive compositions prepared in Examples 1-13 and Comparative Examples 1-3.

[0088] The preparation process of application examples 1-13 and comparative application examples 1-3 is as follows:

[0089] The flame retardant adhesive composition is coated on one side of the polyimide film, and dried at a temperature of 120° C. for 8 minutes; and rolled up after natural cooling to obtain a flame retardant tape.

[0090] Performance Testing

[0091] The flame retardant tapes prepared in Application Examples 1-13 and Comparative Examples 1-3 were subjected to the following performance tests:

[0092] (1) The bonding properties (N / mm) of the flame retardant tapes prepared in Application Examples 1-13 and Comparative Application Examples 1-3 were measured with reference to standard GB / T 4851-2003.

[0093] (2) The breakdown voltage (Kv) of the flame retardant tapes prepared in Application Examples 1-13 and Comparative Examples 1-3 was determined with reference to standard GB / T 1408.1-2017.

[0094] (3) The flame retardant properties of the flame retardant tapes prepared in Application Examples 1-13 and Comparative Application Examples 1-3 were determined in accordance with standard GB / T 2408-2008.

[0095] (4) The smoke density of the flame retardant tapes prepared in Application Examples 1-13 and Comparative Examples 1-3 was measured with reference to Standard GB8323-87.

[0096] (5) The oxygen index of the flame retardant tapes prepared in Application Examples 1-13 and Comparative Examples 1-3 was determined with reference to standard GB / T2406-2008.

[0097] The measurement results are shown in Tables 2 and 3.

[0098] Table 2

[0099]

[0100]

[0101] Table 3

[0102] Smoke density (Ds) Oxygen index (%) Is it burning and dripping? Application Example 1 21 33.2 No dripping Application Example 2 19 34.7 No dripping Application Example 3 22 34.1 No dripping Application Example 4 24 32.8 No dripping Application Example 5 22 33.4 No dripping Application Example 6 24 33.5 No dripping Application Example 7 22 32.7 No dripping Application Example 8 27 29.8 A small amount of dripping Application Example 9 26 28.4 No dripping Application Example 10 23 30.5 No dripping Application Example 11 20 33.1 No dripping Application Example 12 26 29.4 A small amount of dripping Application Example 13 15 36.9 No dripping Application Comparative Example 1 35 23.5 Dripping Application Comparative Example 2 46 22.6 A small amount of dripping Application Comparative Example 3 31 25.2 A small amount of dripping

[0103] By comparing and analyzing the data in Table 2 and Table 3, internally comparing Application Examples 1-13, and comparing Application Examples 1-13 with Application Comparative Examples 1-3, it can be found that the flame retardant tape prepared in Application Example 13 has the best post-combustion expansion and smoke suppression effects, and can completely achieve no dripping and no obvious smoke generation during the combustion process. Therefore, the present application provides a highly efficient halogen-free flame retardant flame retardant adhesive composition and flame retardant tape, which have the characteristics of good flame retardant effect, anti-dripping, low smoke emission, excellent bonding performance, etc., simple preparation process, low cost, and suitable for promotion and application.

[0104] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A flame retardant adhesive composition, It is characterized in that The invention comprises the following raw materials in parts by weight: 80-110 parts of epoxy resin, 40-75 parts of acrylic copolymer, 7-13 parts of ammonium polyphosphate, 4-6 parts of carboxymethyl cellulose calcium, 2-4.5 parts of expanded graphite, 6-11 parts of curing agent, 8-16 parts of diluent, and 2-4 parts of defoaming agent; The acrylic copolymer comprises a hydroxypropyl acrylate-acrylic acid copolymer and an isooctyl acrylate-acrylic acid copolymer in a weight ratio of 2-4:5-8; The particle size of the expanded graphite is 0.5-5um.

2. The flame retardant adhesive composition according to claim 1, It is characterized in that The invention comprises the following raw materials in parts by weight: 100 parts of epoxy resin, 55 parts of acrylic polymer, 12 parts of ammonium polyphosphate, 5.5 parts of carboxymethyl cellulose calcium, 4 parts of expanded graphite, 9 parts of curing agent, 10 parts of diluent and 2.5 parts of defoaming agent.

3. The flame retardant adhesive composition according to claim 1, It is characterized in that The curing agent includes one or more of ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, polyetheramine, metaphenylenediamine, diphenylmethanediamine, isophoronediamine and polyamide.

4. The flame retardant adhesive composition according to claim 1, It is characterized in that The expanded graphite is modified expanded graphite, and the preparation method of the modified expanded graphite comprises the following steps: (1) Add acetylferrocene, formaldehyde, sodium hydroxide and potassium carbonate into a container, grind at 15-30°C, wash with water, and dry to obtain ferrocene ketone, which is set aside; (2) 98 wt% concentrated sulfuric acid, hydrogen peroxide and graphite are mixed, reacted for 80-120 min, dried, heat treated, added to an acetone solution of ferrocenyl ketone, ultrasonically dispersed, filtered and dried to obtain modified expanded graphite.

5. A method for preparing the flame retardant adhesive composition according to any one of claims 1 to 4, It is characterized in that The following steps are involved: Mix the epoxy resin, diluent and defoamer, heat to 50-75°C, stir for 0.5-1h, heat to 85-95°C, add expanded graphite and acrylic copolymer, stir for 1-2h; cool to 50-75°C, add the remaining raw materials, stir for 1-2h to obtain a flame retardant adhesive composition.

6. A flame retardant tape, It is characterized in that The invention comprises a substrate and a flame retardant adhesive composition coated on one side of the substrate, wherein the substrate is selected from a polypropylene film, a polyvinyl chloride film, a polyimide film and a polyester film, and the flame retardant adhesive composition is the flame retardant adhesive composition described in any one of claims 1 to 4.

7. A method for preparing the flame retardant tape according to claim 6, It is characterized in that The following steps are involved: The flame retardant adhesive composition is coated on one side of a substrate, dried at a temperature range of 70-140° C., and rolled up after natural cooling to obtain a flame retardant tape.