Epitaxial growth method of iron-doped GaN buffer layer and GaN microwave power device

By using organic metal chemical vapor deposition method to grow the AlN nucleated layer and the iron-doped GaN buffer layer on the SiC substrate, the growth conditions are controlled, and the problems of low resistivity and surface atomization of the buffer layer of the GaN microwave power device on the SiC substrate are solved. , achieves high resistivity and flat surface growth, suitable for large-scale mass production.

CN118422329BActive Publication Date: 2024-11-05JIANGSU CORENERGY SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410895476.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-05
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

The resistivity of the undoped buffer layer of GaN microwave power devices on the SiC substrate is low, resulting in the impact of the device amplifier characteristics, and the buffer layer surface atomization under the high-iron doping concentration is unable to be used for subsequent device structure growth.

Method used

The AlN nucleated layer and iron-doped GaN buffer layer were grown on SiC single crystal substrate by chemical vapor deposition method. The pressure in the reaction chamber was controlled at 600~1000mbar, the V/III ratio was (100~300):1, Fe source The molar flux ratio to the Ga source is between 1E-5 and 1E-3, and the island-like growth mode is suppressed by adjusting the growth conditions to form a continuous smooth surface with high resistivity.

Benefits of technology

While ensuring that the GaN crystal quality remains unchanged, the resistivity of the iron-doped GaN buffer layer is increased, the growth time is extended, suitable for large-scale mass production, and the iron doping amount is increased, from E18cm-3 to E19~E20cm -3, enhances the resistivity of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118422329B_ABST
    Figure CN118422329B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of GaN microwave power devices, and specifically relates to an epitaxial growth method of an iron-doped GaN buffer layer and a GaN microwave power device. The present invention adopts an organic metal chemical vapor deposition method to grow an AlN nucleation layer on a SiC single crystal substrate; then grow an iron-doped GaN buffer layer on the AlN nucleation layer: the pressure of the reaction chamber is 600~1000mbar; the V / III ratio passed into the reaction chamber is (100~300):1; the molar flux ratio of the Fe source and the Ga source is 1E‑5~1E‑3. The epitaxial growth method of the iron-doped GaN buffer layer provided by the present invention is suitable for MOCVD equipment. When growing the iron-doped GaN buffer layer, by adjusting the pressure and V / III ratio of the reaction chamber, and at the same time doping a large amount of Fe elements, the growth of a high-resistivity buffer layer is achieved while ensuring that the quality of the GaN crystal remains unchanged, and it is suitable for large-scale mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of GaN microwave power devices, and in particular relates to an epitaxial growth method of an iron-doped GaN buffer layer and a GaN microwave power device. Background Art

[0002] At present, GaN microwave power devices made on SiC substrates have been widely used in radar T / R modules and 5G base stations. Microwave power devices require that the GaN buffer layer must meet certain insulation properties, and a nanometer-thick oxide layer is easily formed on the surface of the SiC substrate. In the subsequent epitaxial growth process, the oxygen atoms in the oxide on the surface of the SiC substrate will diffuse into the GaN buffer layer, forming shallow donor energy levels in the GaN material. At the same time, there are a large number of nitrogen vacancies in the unintentionally doped GaN material, and this defect will also introduce a large number of shallow donor energy levels. Therefore, under the influence of various factors, the resistivity of the undoped GaN buffer layer on SiC is low, which seriously affects the power amplifier characteristics of the device.

[0003] At present, people generally introduce deep energy levels by adding dopants during the growth process to increase the resistivity of the material. Iron is one of the commonly used doping elements. Another study showed that the O content and dislocation density at the GaN / SiC interface are much higher than those of the bulk material. Therefore, in the initial growth stage of the buffer layer, a larger dose of doping elements is required to compensate for the excess shallow donor energy levels. The traditional growth process is to introduce Ga source and Fe source at the same time under the growth conditions of 100~300mbar and V / III ratio of about 1000. The buffer layer grown under this pressure will first nucleate on the AlN nucleation layer and form an island structure, and then quickly grow and merge laterally to form a smooth and continuous surface morphology in a two-dimensional layered growth mode. When the iron doping concentration is less than about 5E18cm -3 When the Fe doping concentration is greater than about 1E19 cm -3 Afterwards, a large dose of iron changed the surface energy of each crystal face of GaN. Although the buffer layer was also laid flat on the AlN nucleation layer in a two-dimensional layered growth mode in the initial growth stage, after the continuous film layer was formed, it began to show an island growth mode, the quality of GaN crystal deteriorated, and the surface coarsened rapidly with the increase of growth time, which eventually led to the atomization of the buffer layer surface and the low resistivity, making it unusable for the growth of subsequent device structures.

[0004] Chinese patent CN115588615A discloses a method for epitaxial growth of high-mobility AlN / GaN heterojunction materials, but the patent does not disclose solutions to related problems such as buffer layer surface atomization, reduced resistivity, and inability to be used for subsequent device structure growth during epitaxial growth. Summary of the invention

[0005] The purpose of the present invention is to provide an epitaxial growth method of an iron-doped GaN buffer layer and a GaN microwave power device. The method provided by the present invention can achieve the growth of a high-resistivity iron-doped GaN buffer layer while ensuring that the quality of GaN crystals in the iron-doped GaN buffer layer remains unchanged.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides an epitaxial growth method of an Fe-doped GaN buffer layer, comprising the following steps:

[0008] An AlN nucleation layer is grown on a SiC single crystal substrate by an organic metal chemical vapor deposition method; then an iron-doped GaN buffer layer is grown on the AlN nucleation layer; the conditions for growing the iron-doped GaN buffer layer include: a pressure in a reaction chamber of 600-1000 mbar; an N source, a Ga source and an Fe source are passed into the reaction chamber; a molar flux ratio of the N element in the N source to the Ga element in the Ga source is (100-300):1; and a molar flux ratio of the Fe element in the Fe source to the Ga element in the Ga source is 1E-5-1E-3.

[0009] Preferably, the conditions for growing the Fe-doped GaN buffer layer also include: the temperature of the reaction chamber is 900-1000° C.; and the Ga source and the Fe source are introduced into the reaction chamber at the same time.

[0010] Preferably, the N source includes NH3; the Fe source includes ferrocene; and the Ga source includes trimethylgallium and / or triethylgallium.

[0011] Preferably, the thickness of the iron-doped GaN buffer layer is 0.3-1 μm; the doping amount of Fe element in the iron-doped GaN buffer layer is 1E19-1E20 cm -3 .

[0012] Preferably, the conditions for growing the AlN nucleation layer include: the pressure of the reaction chamber is 50-100 mbar, the temperature is 1100-1150° C.; an Al source and a N source are introduced simultaneously;

[0013] The thickness of the AlN nucleation layer is 30-100 nm.

[0014] The present invention provides an epitaxial growth method of a GaN microwave power device, wherein the GaN microwave power device comprises a SiC single crystal substrate and an AlN nucleation layer, an Fe-doped GaN buffer layer, a non-doped GaN channel layer, an AlN insertion layer, an AlGaN barrier layer and a GaN cap layer which are sequentially stacked on the surface of the SiC single crystal substrate; the method comprises the following steps:

[0015] An AlN nucleation layer, an Fe-doped GaN buffer layer, a non-doped GaN channel layer, an AlN insertion layer, an AlGaN barrier layer and a GaN cap layer are sequentially grown on the SiC single crystal substrate by an organic metal chemical vapor deposition method;

[0016] The AlN nucleation layer and the Fe-doped GaN buffer layer are prepared according to the epitaxial growth method described in the above technical solution.

[0017] Preferably, the conditions for growing the non-doped GaN channel layer include: the pressure of the reaction chamber is 200-300 mbar, and the temperature is 1000-1050° C.;

[0018] The thickness of the non-doped GaN channel layer is 0.5-1.5 μm.

[0019] Preferably, the conditions for growing the AlN insertion layer include: the pressure of the reaction chamber is 50-150 mbar and the temperature is 1000-1050° C.;

[0020] The thickness of the AlN insertion layer is 0.5-1.5 nm.

[0021] Preferably, the conditions for growing the AlGaN barrier layer include: the pressure of the reaction chamber is 50-150 mbar, and the temperature is 1000-1050° C.;

[0022] The thickness of the AlGaN barrier layer is 10-25 nm; the chemical composition of the AlGaN barrier layer is Al x Ga 1-x The molar ratio of N, Al element, Ga element and N element is x:(1-x):1, wherein x is 0.1~0.3.

[0023] Preferably, the conditions for growing the GaN cap layer include: the pressure of the reaction chamber is 50-150 mbar and the temperature is 1000-1050° C.;

[0024] The thickness of the GaN cap layer is 1-3 nm.

[0025] The invention provides an epitaxial growth method of an iron-doped GaN buffer layer, comprising the following steps: growing an AlN nucleation layer on a SiC single crystal substrate by an organic metal chemical vapor deposition method; then growing an iron-doped GaN buffer layer on the AlN nucleation layer; conditions for growing the iron-doped GaN buffer layer comprising: a pressure in a reaction chamber of 600-1000 mbar; passing an N source, a Ga source and an Fe source into the reaction chamber; a molar flux ratio (V / III ratio) of an N element in the N source to a Ga element in the Ga source of (100-300):1; and a molar flux ratio of an Fe element in a Fe source to a Ga element in a Ga source of 1E-5-1E-3. Since the Fe element changes the surface energy of each crystal plane of GaN, resulting in a change in the isotropic growth rate, the present invention effectively changes the growth mode of the initial growth stage of the iron-doped GaN buffer layer by controlling the pressure conditions and V / III ratio of the iron-doped GaN buffer layer grown by the metal organic chemical vapor deposition method, and can effectively inhibit the island growth mode of the GaN buffer layer during the growth process when a large dose of iron is doped (i.e., the molar flux ratio of the Fe element in the Fe source and the Ga element in the Ga source is 1E-5~1E-3), forming a continuous and smooth surface morphology, thereby growing a high-resistance buffer layer that can be used for microwave radio frequency devices. In summary, the epitaxial growth method of the iron-doped GaN buffer layer provided by the present invention is suitable for metal organic chemical vapor deposition (MOCVD) equipment. When growing the iron-doped GaN buffer layer, the pressure of the reaction chamber (close to normal pressure) and the growth environment of the V / III ratio (extremely low V / III ratio) are adjusted, and a large amount of Fe elements are doped at the same time, so as to achieve the growth of a high-resistivity buffer layer while ensuring that the quality of the GaN crystal remains unchanged. It can be seen from the results of the examples that compared with the prior art, the present invention can further increase the iron doping amount in the buffer layer on the basis of ensuring the surface flatness and crystal quality of the buffer layer, and can increase the iron doping amount in the buffer layer from E18cm -3 The magnitude is increased to E19~E20cm -3 The growth method provided by the present invention has low requirements on equipment process capability and is suitable for large-scale mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A schematic diagram of the structure of the GaN microwave power device provided by the present invention;

[0027] Figure 1 Middle: 1 is SiC single crystal substrate, 2 is AlN nucleation layer, 3 is Fe-doped GaN buffer layer, 4 is non-doped GaN channel layer, 5 is AlN insertion layer, 6 is AlGaN barrier layer, and 7 is GaN cap layer;

[0028] Figure 2 This is an AFM photograph of an iron-doped GaN buffer layer prepared in an embodiment of the present invention;

[0029] Figure 3 This is an OM photograph of the surface morphology of the iron-doped GaN buffer layer prepared in an embodiment of the present invention;

[0030] Figure 4 It is a comparison diagram of the growth reflectivity curves of the conventional process of Comparative Example 1 and the optimized process of Example 1;

[0031] Figure 5 This is a comparison chart of the withstand voltage curves of the iron-doped GaN buffer layer prepared by the conventional process of Comparative Example 1 and the optimized process of Example 1. DETAILED DESCRIPTION

[0032] The present invention provides an epitaxial growth method of an Fe-doped GaN buffer layer, comprising the following steps:

[0033] An AlN nucleation layer is grown on a SiC single crystal substrate by an organic metal chemical vapor deposition method; then an iron-doped GaN buffer layer is grown on the AlN nucleation layer; the conditions for growing the iron-doped GaN buffer layer include: a pressure in a reaction chamber of 600-1000 mbar; an N source, a Ga source and an Fe source are passed into the reaction chamber; a molar flux ratio of the N element in the N source to the Ga element in the Ga source is (100-300):1; and a molar flux ratio of the Fe element in the Fe source to the Ga element in the Ga source is 1E-5-1E-3.

[0034] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0035] The present invention preferably places the SiC single crystal substrate on a MOCVD epitaxial growth base to grow the AlN nucleation layer. Before growing the AlN nucleation layer, the present invention preferably cleans the SiC single crystal substrate to remove contamination on the surface of the SiC single crystal substrate. The cleaning conditions include: the reaction chamber pressure is preferably 50~150mbar, more preferably 100mbar; the temperature is preferably 1000~1100℃, more preferably 1050℃; H2 is introduced into the reaction chamber, and the time for baking the SiC single crystal substrate in the H2 atmosphere is preferably 5~15min, more preferably 10min.

[0036] After cleaning, the present invention grows an AlN nucleation layer on the cleaned SiC single crystal substrate. The conditions for growing the AlN nucleation layer preferably include: the pressure of the reaction chamber is preferably 50-100 mbar, preferably 100 mbar; the temperature is preferably 1100-1150°C; an Al source and a N source are simultaneously introduced into the reaction chamber; the Al source is preferably trimethylaluminum. Trimethylaluminum is a liquid with a high saturated vapor pressure. The present invention uses H2 or N2 as a carrier gas to bring the Al source into the reaction chamber. The N source is preferably NH3, and the molar flux ratio (V / III ratio) of the Al element in the Al source and the N element in the N source is preferably 1000-10000, more preferably 2000. The thickness of the AlN nucleation layer is preferably 30-100 nm, more preferably 50 nm. After the growth of the AlN nucleation layer is completed, the Al source is turned off.

[0037] After the growth of the AlN nucleation layer is completed, the nitrogen source atmosphere is maintained, and the present invention grows an iron-doped GaN buffer layer on the AlN nucleation layer. The conditions for growing the iron-doped GaN buffer layer include: passing an N source, a Ga source and an Fe source into the reaction chamber; the Ga source and the Fe source are simultaneously introduced into the reaction chamber. The N source is preferably NH3. The Fe source is preferably ferrocene; the Ga source is preferably trimethylgallium and / or triethylgallium. The pressure of the reaction chamber is 600~1000mbar, preferably 900mbar. The temperature of the reaction chamber is preferably 900~1000℃. The molar flux ratio of the N element in the N source to the Ga element in the Ga source is (100~300):1, preferably 200:1. The molar flux ratio of the Fe element in the Fe source to the Ga element in the Ga source is 1E-5~1E-3, preferably 1E-4. The thickness of the iron-doped GaN buffer layer is preferably 0.3-1 μm, more preferably 0.5 μm; the doping amount of Fe element in the iron-doped GaN buffer layer is preferably 1E19-1E20 cm -3 After the growth of the Fe-doped GaN buffer layer is completed, the Ga source and the Fe source are turned off.

[0038] The present invention provides an epitaxial growth method of a GaN microwave power device, wherein the GaN microwave power device comprises a SiC single crystal substrate and an AlN nucleation layer, an Fe-doped GaN buffer layer, a non-doped GaN channel layer, an AlN insertion layer, an AlGaN barrier layer and a GaN cap layer which are sequentially stacked on the surface of the SiC single crystal substrate; the method comprises the following steps:

[0039] An AlN nucleation layer, an Fe-doped GaN buffer layer, a non-doped GaN channel layer, an AlN insertion layer, an AlGaN barrier layer and a GaN cap layer are sequentially grown on the SiC single crystal substrate by an organic metal chemical vapor deposition method;

[0040] The AlN nucleation layer and the Fe-doped GaN buffer layer are prepared according to the epitaxial growth method described in the above technical solution.

[0041] After the growth of the iron-doped GaN buffer layer is completed, the nitrogen source atmosphere is maintained, and the present invention grows a non-doped GaN channel layer on the iron-doped GaN buffer layer. In the present invention, the conditions for growing the non-doped GaN channel layer preferably include: the pressure of the reaction chamber is preferably 200~300mbar, more preferably 266mbar; the temperature is preferably 1000~1050℃, more preferably 1030℃. A Ga source is introduced into the reaction chamber, and the Ga source is preferably trimethylgallium and / or triethylgallium. The molar flux ratio (V / III ratio) of the Ga element in the Ga source and the N element in the N source is preferably 1000~1500, more preferably 1200. The thickness of the non-doped GaN channel layer is 0.5~1.5μm, more preferably 1.0μm. After the growth of the non-doped GaN channel layer is completed, the Ga source is turned off.

[0042] After the growth of the non-doped GaN channel layer is completed, the nitrogen source atmosphere is maintained, and the present invention grows an AlN insertion layer on the non-doped GaN channel layer. In the present invention, the conditions for growing the AlN insertion layer include: the pressure of the reaction chamber is preferably 50~150mbar, more preferably 100mbar, and the temperature is preferably 1000~1050℃, more preferably 1030℃. An Al source is introduced into the reaction chamber. The Al source is preferably trimethylaluminum, which is a liquid with a high saturated vapor pressure. The present invention uses H2 or N2 as a carrier gas to bring the Al source into the reaction chamber. The molar flux ratio (V / III ratio) of the Al element in the Al source and the N element in the N source is 5000~30000, more preferably 30000. The thickness of the AlN insertion layer is 0.5~1.5nm, more preferably 1nm. After the growth of the AlN insertion layer is completed, the Al source is turned off.

[0043] After the growth of the AlN insertion layer is completed, the nitrogen source atmosphere is maintained, and the present invention grows an AlGaN barrier layer on the AlN insertion layer. In the present invention, the conditions for growing the AlGaN barrier layer preferably include: the pressure of the reaction chamber is preferably 50~150mbar, more preferably 100mbar, and the temperature is preferably 1000~1050℃, more preferably 1030℃. An Al source and a Ga source are introduced into the reaction chamber. The Al source is preferably trimethylaluminum, which is a liquid with a high saturated vapor pressure. In the present invention, the Al source is brought into the reaction chamber by using H2 or N2 as a carrier gas. The Ga source is preferably trimethylgallium and / or triethylgallium. The ratio of the sum of the molar flux of the Al element in the Al source and the Ga element in the Ga source to the molar flux of the N element in the N source (V / III ratio) is preferably 5000~30000, more preferably 10000. The thickness of the AlGaN barrier layer is 10~25nm, more preferably 20nm. In the present invention, the chemical composition of the AlGaN barrier layer is specifically preferably Al x Ga 1-x N, Al / Ga / N molar ratio is x:(1-x):1; wherein x is 0.1-0.3, more preferably 0.25, that is, wherein the Al component is preferably 10-30%, specifically preferably 25%. After the AlGaN barrier layer is grown, the Al source and the Ga source are turned off.

[0044] After the growth of the AlGaN barrier layer is completed, the nitrogen source atmosphere is maintained, and the present invention grows a GaN cap layer on the AlGaN barrier layer. In the present invention, the conditions for growing the GaN cap layer preferably include: the pressure of the reaction chamber is preferably 50~150mbar, more preferably 100mbar, and the temperature is preferably 1000~1050℃, more preferably 1030℃. A Ga source is introduced into the reaction chamber. The Ga source is preferably trimethylgallium or triethylgallium. The molar flux ratio (V / III ratio) of the Ga element in the Ga source and the N element in the N source is 5000~30000, more preferably 15000. The thickness of the GaN cap layer is 1~3nm, more preferably 2nm.

[0045] After the GaN cap layer is grown, the Ga source is turned off. After the epitaxial growth is finished, the present invention cools down in an NH3 atmosphere, and finally takes out the epitaxial wafer to obtain a GaN microwave power device.

[0046] The present invention provides an epitaxial growth method for growing high-quality semi-insulating iron-doped GaN on a SiC substrate. The method is applicable to MOCVD equipment, and when growing an iron-doped GaN buffer layer, the reaction chamber is adjusted to a growth environment close to normal pressure and an extremely low V / III ratio, and a large amount of Fe elements are doped at the same time, so as to achieve the growth of a high-resistivity buffer layer while ensuring that the quality of the GaN crystal remains unchanged.

[0047] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0048] In the following embodiments, GaN microwave power devices are Figure 1 Schematic diagram of the structure shown in the figure

[0049] Example 1

[0050] This embodiment provides a method for growing a high-quality iron-doped GaN buffer layer and a GaN microwave power device on a SiC substrate, which specifically includes the following steps:

[0051] Step 1: Select a SiC single crystal substrate and place it on a MOCVD epitaxial growth base.

[0052] Step 2: Set the reaction chamber pressure to 100 mbar, introduce H2, raise the temperature to 1050°C, bake the substrate in H2 atmosphere for 10 minutes to remove surface contamination; turn off H2.

[0053] Step 3: Set the reaction chamber pressure to 100 mbar, set the molar flux ratio of Al element in the Al source and N element in NH3 (V / III ratio) to 2000, and after heating to 1100°C, introduce Al source (trimethylaluminum) and NH3 at the same time to grow an AlN nucleation layer with a thickness of 50 nm, and turn off the Al source.

[0054] Step 4: Maintaining the NH3 atmosphere, set the molar flux ratio of Ga in the Ga source to N in NH3 (V / III ratio) to 200, set the molar flux ratio of Fe in the Fe source to Ga in the Ga source to 1E-4, set the pressure of the reaction chamber to 900 mbar, lower the temperature to 900 °C, introduce Ga source (trimethylgallium or triethylgallium) and Fe source (ferrocene) at the same time, and grow an Fe-doped GaN buffer layer with a thickness of 0.5 μm, in which the Fe doping amount is 1E19 cm -3 , turn off the Ga source and Fe source. Figure 2 This is an AFM photograph of the iron-doped GaN buffer layer prepared in Example 1 of the present invention. Figure 3 This is an OM photograph of the surface morphology of the Fe-doped GaN buffer layer prepared in Example 1 of the present invention. Figure 2 and Figure 3 It can be seen that the surface flatness of the iron-doped GaN buffer layer prepared in this embodiment is extremely high.

[0055] Step 5: Maintain the NH3 atmosphere, set the molar flux ratio of Ga in the Ga source and N in NH3 (V / III ratio) to 1200, set the pressure of the reaction chamber to 266 mbar, increase the temperature to 1030°C, introduce the Ga source, grow a non-doped GaN channel layer with a growth thickness of 1.0 μm, and turn off the Ga source.

[0056] Step 6: Maintaining the NH3 atmosphere, set the molar flux ratio of Al element in the Al source and N element in NH3 (V / III ratio) to 30000, set the reaction chamber pressure to 100 mbar, keep the temperature constant (1030°C), introduce the Al source (trimethylaluminum, trimethylaluminum is a liquid with high saturated vapor pressure, brought into the reaction chamber by H2 or N2 as a carrier gas), grow the AlN insertion layer, and grow a thickness of 1.0 nm. Turn off the Al source.

[0057] Step 7: Maintaining the NH3 atmosphere, set the ratio of the sum of the molar flux of the Al element in the Al source and the Ga element in the Ga source to the molar flux of the N element in NH3 (V / III ratio) to 10000, set the reaction chamber pressure (100 mbar) and temperature (1030°C) unchanged, introduce the Al source and Ga source, and grow the AlGaN barrier layer with a chemical composition of Al x Ga 1-x N, Al / Ga / N molar ratio is x:(1-x):1; the Al component is 25%, the thickness of the AlGaN barrier layer is 20nm, and the Al source and Ga source are turned off.

[0058] Step 8: Maintaining the NH3 atmosphere, set the molar flux ratio of Ga element in the Ga source and N element in NH3 (V / III ratio) to 15000, set the reaction chamber pressure (100 mbar) and temperature (1030°C) unchanged, introduce the Ga source, grow a GaN cap layer with a thickness of 2 nm, turn off the Ga source, and end the epitaxial growth.

[0059] Step 9: Cool down in an NH3 atmosphere, and finally take out the epitaxial wafer to obtain a GaN microwave power device.

[0060] Comparative Example 1

[0061] The growth method is basically the same as that in Example 1, except that step 4 in Example 1 is replaced as follows:

[0062] Step 4: Keep the NH3 atmosphere unchanged, set the molar flux ratio of Ga in the Ga source and N in NH3 (V / III ratio) to 1000, set the molar flux ratio of Fe in the Fe source to Ga in the Ga source to 3E-6, set the pressure of the reaction chamber to 200 mbar, reduce the temperature to 1050°C, introduce Ga source (trimethylgallium or triethylgallium) and Fe source (ferrocene) at the same time, and grow a 1μm thick Fe-doped GaN buffer layer, in which the Fe doping amount is 1E18cm -3 , turn off the Ga source and Fe source.

[0063] Test example:

[0064] Figure 4 is a comparison chart of the growth reflectivity curves of the conventional process of Comparative Example 1 and the optimized process of Example 1; Figure 4 It can be seen that when the buffer layer is doped with the same 1E19cm-3 Fe dopant, with the introduction of the MO source, the reflectivity of the conventional process drops rapidly to near zero, indicating that the surface of the epitaxial wafer is rapidly coarsened and the surface is fogged; while the reflectivity of the optimized process oscillates up and down with the growth time, indicating that the surface of the epitaxial layer is smooth and grows in a two-dimensional layered manner.

[0065] Figure 5 The comparison diagram of the withstand voltage curves of the Fe-doped GaN buffer layer prepared by the conventional process of Comparative Example 1 and the optimized process of Example 1; Figure 5 It can be seen that the optimized process of Example 1 further increases the iron doping amount in the buffer layer on the basis of ensuring the crystallization quality of the buffer layer, and can increase the iron doping amount in the buffer layer from the order of E18cm-3 of Comparative Example 1 to the order of E19cm-3, thereby further improving the material resistivity. Under the same voltage, the leakage current of the Fe-doped buffer layer of order E19 in Example 1 is smaller.

[0066] From the above embodiments, it can be seen that the conventional preparation process of the current iron-doped GaN buffer layer (Comparative Example 1) is used to grow the GaN buffer layer on the SiC substrate at a common pressure of 100~300mbar and a V / III ratio of 1000. The iron-doped GaN buffer layer grown under this pressure and V / III ratio will first nucleate on the AlN nucleation layer and form an island structure, and then rapidly grow and merge laterally to form a smooth and continuous surface morphology in a two-dimensional layered growth mode. When the iron doping concentration is less than about 5E18cm-3, the growth of the buffer layer follows this growth mode. However, when the iron doping concentration is greater than about 1E19cm-3, a large dose of Fe element changes the surface energy of each crystal face of GaN. Although the iron-doped GaN buffer layer is also laid flat on the AlN nucleation layer in a two-dimensional layered growth mode in the initial growth stage, after forming a continuous film layer, it begins to show an island growth mode, and the surface rapidly coarsens as the growth time increases, which eventually leads to atomization of the buffer layer surface and cannot be used for the growth of subsequent device structures. The present invention adopts process conditions of near-normal pressure and extremely low V / III ratio when preparing the iron-doped GaN buffer layer. The present invention can effectively suppress the island growth mode in the growth process of the high-dose iron-doped GaN buffer layer by adopting a relatively extreme growth process (growth conditions of near-normal pressure and extremely low V / III ratio), forming a continuous and smooth surface morphology, thereby growing a high-resistance buffer layer that can be used for microwave radio frequency devices.

[0067] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for epitaxial growth of an Fe-doped GaN buffer layer, It is characterized in that The following steps are involved: An AlN nucleation layer is grown on a SiC single crystal substrate by an organic metal chemical vapor deposition method; then an Fe-doped GaN buffer layer is grown on the AlN nucleation layer; the conditions for growing the Fe-doped GaN buffer layer include: a pressure in a reaction chamber of 600-1000 mbar; a temperature in the reaction chamber of 900-1000° C.; an N source, a Ga source and an Fe source are introduced into the reaction chamber; a molar flux ratio of the N element in the N source to the Ga element in the Ga source is (100-300):1; a molar flux ratio of the Fe element in the Fe source to the Ga element in the Ga source is 1E-5-1E-3; and a doping amount of the Fe element in the Fe-doped GaN buffer layer is 1E19-1E20 cm -3 .

2. The epitaxial growth method according to claim 1, It is characterized in that The conditions for growing the Fe-doped GaN buffer layer also include: the Ga source and the Fe source are introduced into the reaction chamber at the same time.

3. The epitaxial growth method according to claim 1 or 2, It is characterized in that The N source includes NH 3 ; The Fe source includes ferrocene; The Ga source includes trimethylgallium and / or triethylgallium.

4. The epitaxial growth method according to claim 1 or 2, It is characterized in that The thickness of the iron-doped GaN buffer layer is 0.3-1 μm.

5. The epitaxial growth method according to claim 1, It is characterized in that The conditions for growing the AlN nucleation layer include: the pressure of the reaction chamber is 50-100 mbar, the temperature is 1100-1150° C.; an Al source and a N source are introduced simultaneously; The thickness of the AlN nucleation layer is 30-100 nm.

6. A method for epitaxial growth of a GaN microwave power device, the GaN microwave power device comprising a SiC single crystal substrate and an AlN nucleation layer, an Fe-doped GaN buffer layer, a non-doped GaN channel layer, an AlN insertion layer, an AlGaN barrier layer and a GaN cap layer stacked in sequence on the surface of the SiC single crystal substrate; It is characterized in that The following steps are involved: An AlN nucleation layer, an Fe-doped GaN buffer layer, a non-doped GaN channel layer, an AlN insertion layer, an AlGaN barrier layer and a GaN cap layer are sequentially grown on the SiC single crystal substrate by an organic metal chemical vapor deposition method; The AlN nucleation layer and the Fe-doped GaN buffer layer are prepared according to the epitaxial growth method according to any one of claims 1 to 5.

7. The epitaxial growth method according to claim 6, It is characterized in that The conditions for growing the non-doped GaN channel layer include: the pressure of the reaction chamber is 200-300 mbar and the temperature is 1000-1050° C.; The thickness of the non-doped GaN channel layer is 0.5-1.5 μm.

8. The epitaxial growth method according to claim 6, It is characterized in that The conditions for growing the AlN insertion layer include: the pressure of the reaction chamber is 50-150 mbar and the temperature is 1000-1050° C.; The thickness of the AlN insertion layer is 0.5-1.5 nm.

9. The epitaxial growth method according to claim 6, It is characterized in that The conditions for growing the AlGaN barrier layer include: a reaction chamber pressure of 50-150 mbar and a temperature of 1000-1050° C.; The thickness of the AlGaN barrier layer is 10-25 nm; the chemical composition of the AlGaN barrier layer is Al x Ga 1-x The molar ratio of N, Al element, Ga element and N element is x:(1-x):1, wherein x is 0.1~0.

3.

10. The epitaxial growth method according to claim 6, It is characterized in that The conditions for growing the GaN cap layer include: a reaction chamber pressure of 50-150 mbar and a temperature of 1000-1050° C.; The thickness of the GaN cap layer is 1-3 nm.