High-strength and high-elongation aluminum alloy rod and preparation method and application thereof

By adjusting the composition and process of aluminum alloy, the problem of insufficient tensile strength and elongation of aluminum rods was solved, and high-strength high-elongation aluminum alloy rods were prepared, which were suitable for high-voltage transmission projects and improved cable performance.

CN118979166APending Publication Date: 2024-11-19JIANGSU HENGTONG ELECTRICAL SPECIAL WIRE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411075634.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing aluminum rods have poor performance in tensile strength and elongation, resulting in insufficient performance in high-voltage or ultra-high voltage transmission projects and cannot meet the requirements for improving cable performance.

Method used

By adjusting the composition ratio of aluminum alloy and improving production processes, including borication treatment, multiple refining, addition of aluminum-titanium boron wire, casting and rolling, the Fe/Si ratio, the use of rare earth elements, and the temperature and pressure. To improve the tensile strength and elongation of aluminum alloy rods.

Benefits of technology

The preparation of high-strength high-elongation aluminum alloy rods was achieved, the tensile strength was increased to 100-110MPa, the elongation reached 20-25%, and the excellent conductivity and performance were shown in cable monofilament applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a high-strength and high-elongation aluminum alloy rod and a preparation method and application thereof.The preparation method comprises the steps of smelting, boronizing treatment, primary refining, corresponding alloy adding, secondary refining, degassing and filtering, continuous casting and rolling treatment, and the high-strength and high-elongation aluminum alloy rod is prepared from 0.03 wt%-0.05 wt% of Si, 0.25 wt%-0.35 wt% of Fe, 0.02 wt%-0.04 wt% of Ce, 0.01 wt%-0.02 wt% of La, 0.005 wt%-0.015 wt% of Y, 0.002 wt%-0.010 wt% of Ti, 0.001 wt%-0.002 wt% of Cr + Mn + V and the balance Al and inevitable impurities. And the ratio of Fe to Si is larger than or equal to 5 and smaller than or equal to 10, and the high-strength and high-elongation aluminum alloy rod with the tensile strength being 100-110 MPa, the electric conductivity being 61.80-62.06% and the elongation being 20-25% is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy materials, and in particular to a high-strength and high-elongation aluminum alloy rod and a preparation method and application thereof. Background Art

[0002] Electrical round aluminum rods are mainly used to produce power cable products. With the continuous increase in demand for electricity, the requirements for the performance of wires and cables have become higher. Not only are the requirements for the electrical conductivity of electrical round aluminum tubes increased, but also higher requirements have been made for tensile strength and elongation. At present, the grains of ordinary aluminum rods are coarse, which has a great impact on strength, elongation and resistance. The elongation of ordinary A6 aluminum rods is only 10% to 13%. In terms of the single-filament performance of ordinary cables, the conductivity is between 61.7 and 62.0% IACS, the tensile strength is between 175 and 180 MPa, and the elongation is between 1.0 and 1.2%. The strength is low, the overhead wire cross-sectional area is large, the sag is large, the wire span distance is limited, and the elongation is poor. It will affect the performance and life of the cable during production and use, so it is not suitable for large-span, high-voltage or ultra-high-voltage transmission projects. Therefore, it is of great significance to develop a high-strength and high-elongation aluminum alloy rod. Summary of the invention

[0003] In order to solve the above technical problems, the purpose of the present invention is to provide a high-strength and high-elongation aluminum alloy rod and its preparation method and application. By adjusting the component ratio and improving the production process, the elongation is improved to a higher level while ensuring sufficient tensile strength and qualified resistivity.

[0004] The above object of the present invention is achieved through the following technical solutions:

[0005] A first aspect of the present invention provides a method for preparing a high-strength and high-elongation aluminum alloy rod, comprising the following steps:

[0006] S1. Smelting the aluminum alloy in a smelting furnace, performing a boronization treatment, and refining once to obtain a first aluminum liquid;

[0007] S2. The first aluminum liquid obtained in S1 is transferred to a holding furnace, the composition of the first aluminum liquid is detected, and the corresponding alloy is added to obtain a second aluminum liquid, wherein the second aluminum liquid contains Si 0.03-0.05wt%, Fe 0.25-0.35wt%, Ce 0.02-0.04wt%, La 0.01-0.02wt%, Y 0.005-0.015wt%, Ti 0.002-0.010wt%, Cr+Mn+V 0.001-0.002wt%, and the rest is Al and unavoidable impurities, and the Fe / Si ratio is 5≤Fe / Si≤10;

[0008] S3. The second aluminum liquid obtained in S2 is subjected to secondary refining to obtain a third aluminum liquid;

[0009] S4. Aluminum titanium boron wire is added to the third aluminum liquid obtained in S3, and the fourth aluminum liquid is obtained after degassing and filtering;

[0010] S5. The fourth aluminum liquid obtained in S4 is continuously cast at a casting temperature of 680 to 700°C and a casting speed of 6.5 to 7.5 t / h to obtain a continuous billet;

[0011] S6. The continuous billet obtained in S5 is rolled at a rolling temperature of 450-490°C. During the rolling process, the aluminum rod and the rolling mill are lubricated and cooled by controlling the pressure and temperature of the emulsion. The rod closing temperature is 310-350°C. After cooling to 20-30°C, a high-strength and high-elongation aluminum alloy rod is obtained.

[0012] For the Fe / Si ratio in the formula, when the Fe / Si ratio is between 3 and 5, the tensile strength will increase with the increase of the Fe / Si ratio. However, when Fe / Si is greater than or equal to 5, the number of cast second phases increases significantly, and the coarse needle-like FeAl3 phase increases, which is harmful to the performance. In order to eliminate this effect, rare earth Ce can be added to change the form of Fe in the melt, which can eventually narrow the crystallization temperature range and reduce the crack tendency. When the Fe content is lower than 0.21%, a granular α-Fe phase is preferentially formed. When the Fe content is in the range of 0.21% to 1.24%, with the increase of the Fe content, a dense polygonal primary iron phase is formed, and the size increases, which further leads to a decrease in the elongation of the material. In addition, the increase in the iron content in the material will increase the solid solution iron content, which can increase the work hardening rate, thereby ensuring that a higher tensile strength is obtained after subsequent work hardening.

[0013] The various compounds formed by rare earth elements, the adsorption of rare earths at the interface and the solid solution strengthening of the α matrix are also the reasons for the improvement of alloy strength. Among them, the Ce element has a strong purifying effect on the Fe and Si impurities in the aluminum matrix, forming Al-Fe-Si-Ce compounds instead of solid solutions in the aluminum matrix, which is beneficial to improve the resistivity and strength. A trace amount of La can greatly refine the matrix, and similar to the modifiers Na and Sr, it affects the growth behavior of eutectic Si by inducing staggered twins and increasing the twin density, transforming the coarse lamellar eutectic Si into small short rods. A small amount of La addition refines the α-Al grains by reducing the wetting angle between the nucleation site and the α-Al nucleus, and by absorbing Al 13 Fe4 growth edge and poisons the oriented growth to change Al 13 Fe4 minority phase. Grain refinement, Al 13The modification of the Fe4 intermetallic phase and the reduction of the solubility of Fe and Si elements in α-Al induce the enhancement of strength and plasticity, respectively, thereby effectively improving the mechanical properties of the alloy. La and Y play a refining role. The reason for refining the primary silicon crystal is their adsorption on the silicon surface. The rare earth adsorbed on the surface of the primary silicon crystal can effectively inhibit the growth of the primary silicon crystal, increase supercooling, and refine the primary silicon crystal. When the La content is too high, it is easy to aggregate and grow into La-rich compounds, which makes the La around the primary silicon crystal depleted, and the insufficient adsorption causes the primary silicon crystal to coarsen. Y can prevent the formation of coarse lanthanum-rich compounds, thereby improving the lanthanum depletion and refining the primary silicon crystal.

[0014] Furthermore, in S1, boronization treatment is performed by adding aluminum-boron alloy.

[0015] When aluminum-boron alloy is used for boriding treatment, the B element reacts more completely with impurity elements such as Cr, Mn, V, and Ti, thereby reducing the content of impurity elements in the aluminum melt and improving the conductivity.

[0016] Furthermore, in S1, the temperature of the primary refining is 780-800°C.

[0017] Furthermore, in S1, primary refining is performed by blowing nitrogen into the refining agent.

[0018] Furthermore, in S2, the temperature in the insulation furnace is 740-780°C.

[0019] Furthermore, in S3, the temperature of the secondary refining is 740-780°C.

[0020] Furthermore, in S3, secondary refining is performed by blowing in a refining agent using argon gas.

[0021] Furthermore, in S4, the third aluminum liquid in the insulation furnace is poured into the launder, and aluminum titanium boron wire is added before entering the degassing box, and then degassing and filtering are performed in sequence through the degassing box and the filter box.

[0022] Aluminum, titanium and boron can form a solid solution with aluminum, which can refine the grains of aluminum alloys and increase the number of grain boundaries, thereby improving the strength and toughness of the material. The Ti element can significantly refine the grains at a lower content. The effect of a higher content of Ti on improving the elongation is similar to that of adding a small amount of Ti. However, too high a Ti content will significantly increase the resistivity, which is not conducive to improving product performance.

[0023] Furthermore, in S5, during the continuous casting process, the cooling water temperature is 20-40°C, and the billet outlet temperature is 460-500°C.

[0024] Furthermore, in S6, the rolling temperature of the continuous billet is controlled at 450-470°C by turning on the cooling water.

[0025] Furthermore, in S6, the pressure of the emulsion is 195-205 MPa, and the temperature of the emulsion is 60-65°C.

[0026] Furthermore, in S6, the diameter of the high-strength and high-elongation aluminum alloy rod is 9 to 10 mm.

[0027] The present invention adjusts the parameters of casting, rolling mill and emulsion to reduce a certain proportion of work hardening, thereby ensuring high strength and improving the elongation performance of the product.

[0028] The second aspect of the present invention provides a high-strength and high-elongation aluminum alloy rod obtained by the preparation method described in the first aspect.

[0029] The high-strength and high-elongation aluminum alloy rod provided by the invention has a tensile strength of 100-110 MPa, a conductivity of 61.80-62.06%, and an elongation of 20-25%.

[0030] The third aspect of the present invention provides the use of the high-strength and high-elongation aluminum alloy rod described in the second aspect in the preparation of cable monofilaments.

[0031] The invention obtains the cable monofilament by cold drawing the high-strength and high-elongation aluminum alloy rod, wherein the deformation amount of each cold drawing is 10% to 15%, and the monofilament can be drawn to 2.6 to 4.0 mm through multiple drawing passes.

[0032] Beneficial effects of the present invention:

[0033] 1. The high-strength and high-elongation aluminum alloy rod provided by the present invention has the following component contents: Si 0.03-0.05wt%, Fe 0.25-0.35wt%, Ce 0.02-0.04wt%, La 0.01-0.02wt%, Y 0.005-0.015wt%, Ti 0.002-0.010wt%, Cr+Mn+V 0.001-0.002wt%. Ce and La contents within this range have a greater effect on improving strength and elongation. Excessive increase in the rare earth element content has no obvious help in improving elongation and will increase resistivity.

[0034] 2. The preparation method provided by the present invention adopts a triple purification method: first, aluminum-boron alloy is used in a smelting furnace for boronization and primary refining; second, secondary refining is performed in a heat-insulating furnace; third, the aluminum liquid is purified once again in a degassing box and a filter box through a launder. DETAILED DESCRIPTION

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0036] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0037] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0038] The contents of the aluminum alloy rods prepared in the following examples and comparative examples were tested using a SPECTROCHECK direct reading spectrometer.

[0039] The performance of the aluminum alloy rods and aluminum alloy monofilaments prepared in the following examples and comparative examples was tested according to GB / T3954-2022.

[0040] Example 1

[0041] A method for preparing a high-strength and high-elongation aluminum alloy rod comprises the following steps:

[0042] S1. Add an aluminum alloy with a purity of not less than 99.7% into a smelting furnace, heat and melt it, add an aluminum-boron alloy to remove V in the aluminum liquid, keep it warm at 790°C, blow in a refining agent, and perform a refining with nitrogen to obtain the first aluminum liquid.

[0043] S2. The first aluminum liquid obtained in S1 is transferred to a 760°C insulation furnace, and is sampled and tested after standing for 20 minutes. The corresponding Fe, Ce, La, Y and other intermediate alloys are added to the insulation furnace according to the components detected by the direct reading spectrometer, and the second aluminum liquid is obtained after stirring and standing.

[0044] S3. After the second aluminum liquid is tested to be qualified, argon gas is blown into the refining agent and the second refining is carried out at 760°C. After standing, the slag is removed and the third aluminum liquid is obtained by standing for another 35 minutes.

[0045] S4. Pour the third aluminum liquid in the insulation furnace into the flow chute, feed the aluminum titanium boron wire at a speed of 1.5m / s before entering the degassing box, and then degas and filter through the degassing box and the filter box to obtain the fourth aluminum liquid.

[0046] S5. The fourth aluminum liquid obtained in S4 is continuously casted, and the continuous casting conditions are: casting temperature is 690°C, casting speed is 6.7t / h, cooling water temperature is 30°C, billet discharge temperature is 480°C, and continuous billets are obtained.

[0047] S6. The continuous billet obtained in S5 is rolled to obtain an aluminum rod, wherein the aluminum rod has a nominal diameter of 9.5 mm, and the billet rolling temperature is controlled to be 460°C. During the rolling process, the pressure of the emulsion is controlled to be 200 MPa and the temperature is controlled to be 60°C, the aluminum rod and the rolling mill are lubricated and cooled, and the rod closing temperature is 320°C. After the aluminum rod is off the line, it is cooled to room temperature by a fan to obtain the high-strength and high-elongation aluminum alloy rod.

[0048] The element contents of the high-strength and high-elongation aluminum alloy rod were measured to be: Si 0.04wt%, Fe 0.30wt%, Ce 0.03wt%, La 0.01wt%, Y 0.01wt%, Ti 0.007wt%, and Cr+Mn+V 0.002wt%.

[0049] Example 2

[0050] A method for preparing a high-strength and high-elongation aluminum alloy rod is basically the same as Example 1, except that: the intermediate alloy added in S2 is adjusted, and the element content of the high-strength and high-elongation aluminum alloy rod is finally measured to be: Si 0.04wt%, Fe 0.35wt%, Ce 0.04wt%, La 0.02wt%, Y 0.015wt%, Ti 0.007wt%, Cr+Mn+V0.002wt%.

[0051] Example 3

[0052] A method for preparing a high-strength and high-elongation aluminum alloy rod is basically the same as Example 1, except that: the intermediate alloy added in S2 is adjusted, and the element content of the high-strength and high-elongation aluminum alloy rod is finally measured to be: Si 0.04wt%, Fe 0.25wt%, Ce 0.02wt%, La 0.01wt%, Y 0.005wt%, Ti 0.003wt%, Cr+Mn+V0.002wt%.

[0053] Example 4

[0054] A method for preparing a high-strength and high-elongation aluminum alloy rod is basically the same as that of Example 1, except that in S6, the billet rolling temperature is controlled to be 490°C.

[0055] Comparative Example 1

[0056] A method for preparing an aluminum alloy rod is basically the same as that of Example 1, except that the intermediate alloy added to S2 is adjusted, and the element content of the aluminum alloy rod is finally measured to be: Si 0.04wt%, Fe 0.16wt%, Cr+Mn+V0.002wt%.

[0057] Comparative Example 2

[0058] A method for preparing an aluminum alloy rod is basically the same as that of Example 1, except that the intermediate alloy added to S2 is adjusted, and the element content of the aluminum alloy rod is finally measured to be: Si 0.04wt%, Fe 0.16wt%, Ce 0.03wt%, La0.01wt%, Y 0.01wt%, Ti 0.007wt%, Cr+Mn+V 0.002wt%.

[0059] Comparative Example 3

[0060] A method for preparing an aluminum alloy rod is basically the same as that of Example 1, except that the intermediate alloy added to S2 is adjusted, and the element content of the aluminum alloy rod is finally measured to be: Si 0.04wt%, Fe 0.45wt%, Ce 0.03wt%, La0.01wt%, Y 0.01wt%, Ti 0.007wt%, Cr+Mn+V 0.002wt%.

[0061] Comparative Example 4

[0062] A method for preparing an aluminum alloy rod is basically the same as that of Example 1, except that the intermediate alloy added to S2 is adjusted, and the element content of the aluminum alloy rod is finally measured to be: Si 0.04wt%, Fe 0.30wt%, Cr+Mn+V0.002wt%.

[0063] Comparative Example 5

[0064] A method for preparing an aluminum alloy rod is basically the same as that of Example 1, except that the intermediate alloy added to S2 is adjusted, and the element content of the aluminum alloy rod is finally measured to be: Si 0.04wt%, Fe 0.30wt%, Ce 0.06wt%, La0.02wt%, Y 0.02wt%, Ti 0.007wt%, Cr+Mn+V 0.002wt%.

[0065] Comparative Example 6

[0066] A method for preparing an aluminum alloy rod is basically the same as that of Example 1, except that in S5, the casting speed is 6.3 t / h.

[0067] The aluminum alloy rods prepared in the above examples and comparative examples were cold drawn to obtain cable monofilaments, with each cold drawing causing a deformation of 10% to 15%, and the monofilaments were drawn to a diameter of 2.85 mm after multiple passes.

[0068] The element contents of the aluminum alloy rods prepared in Examples 1 to 4 and Comparative Examples 1 to 6 are shown in Table 1:

[0069] Table 1

[0070] Si Fe Ce La Y Ti Cr+Mn+V Example 1 0.04 0.30 0.03 0.01 0.01 0.007 0.002 Example 2 0.04 0.35 0.04 0.02 0.015 0.007 0.002 Example 3 0.04 0.25 0.02 0.01 0.005 0.003 0.002 Example 4 0.04 0.30 0.03 0.01 0.01 0.007 0.002 Comparative Example 1 0.04 0.16 0 0 0 0 0.002 Comparative Example 2 0.04 0.16 0.03 0.01 0.01 0.007 0.002 Comparative Example 3 0.04 0.45 0.03 0.01 0.01 0.007 0.002 Comparative Example 4 0.04 0.30 0 0 0 0 0.002 Comparative Example 5 0.04 0.30 0.06 0.02 0.02 0.007 0.002 Comparative Example 6 0.04 0.30 0.03 0.01 0.01 0.007 0.002

[0071] The properties of the aluminum alloy rods and cable monofilaments prepared in Examples 1 to 4 and Comparative Examples 1 to 6 are shown in Table 2:

[0072] Table 2

[0073]

[0074]

[0075] Comparison between Examples 1 to 3 and Comparative Example 1 shows that adding a certain amount of Fe, Ce, La, Y and Ti elements is beneficial to improving the tensile strength and elongation of the material. Compared with Example 1, Example 4 shows that the control of the rolling temperature is also beneficial to the performance of the product. Compared with Example 1, Comparative Examples 2 and 3 show that increasing the content of Fe elements by a certain amount can improve the strength of the material, but the improvement in strength is not linear. Too high a content of Fe elements will also reduce the elongation of the material. Compared with Example 1, Comparative Example 4 shows that adding a certain amount of rare earth can improve the elongation of the material. Compared with Examples 1 to 3, Comparative Example 5 shows that a certain rare earth content can improve the elongation, while an excessive amount of rare earth will slowly reduce the elongation. Compared with Example 1, Comparative Example 6 shows that maintaining a suitable casting speed is beneficial to product performance.

[0076] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a high-strength and high-elongation aluminum alloy rod, It is characterized in that The following steps are involved: S1. Smelting the aluminum alloy in a smelting furnace, performing a boronization treatment, and refining once to obtain a first aluminum liquid; S2. The first aluminum liquid obtained in S1 is transferred to a holding furnace, the composition of the first aluminum liquid is detected, and the corresponding alloy is added to obtain a second aluminum liquid, wherein the second aluminum liquid contains 0.03-0.05wt% Si, 0.25-0.35wt% Fe, 0.02-0.04wt% Ce, 0.01-0.02wt% La, 0.005-0.015wt% Y, 0.002-0.010wt% Ti, 0.001-0.002wt% Cr+Mn+V, and the rest is Al and unavoidable impurities, and the Fe / Si ratio is 5≤≤10; S3. The second aluminum liquid obtained in S2 is subjected to secondary refining to obtain a third aluminum liquid; S4. Aluminum titanium boron wire is added to the third aluminum liquid obtained in S3, and the fourth aluminum liquid is obtained after degassing and filtering; S5. The fourth aluminum liquid obtained in S4 is continuously cast at a casting temperature of 680 to 700°C and a casting speed of 6.5 to 7.5 t / h to obtain a continuous billet; S6. The continuous billet obtained in S5 is rolled at a rolling temperature of 450-490°C. During the rolling process, the aluminum rod and the rolling mill are lubricated and cooled by controlling the pressure and temperature of the emulsion. The rod closing temperature is 310-350°C. After cooling to 20-30°C, a high-strength and high-elongation aluminum alloy rod is obtained.

2. The preparation method according to claim 1, It is characterized in that In S1, boronization treatment is performed by adding aluminum-boron alloy.

3. The preparation method according to claim 1, It is characterized in that In S1, the primary refining temperature is 780-800°C.

4. The preparation method according to claim 1, It is characterized in that In S2, the temperature in the holding furnace is 740-780°C.

5. The preparation method according to claim 1, It is characterized in that In S3, the temperature of the secondary refining is 740-780°C.

6. The preparation method according to claim 1, It is characterized in that In S5, during the continuous casting process, the cooling water temperature is 20-40°C, and the billet outlet temperature is 460-500°C.

7. The preparation method according to claim 1, It is characterized in that In S6, the pressure of the emulsion is 195-205 MPa, and the temperature of the emulsion is 60-65°C.

8. The preparation method according to claim 1, It is characterized in that In S6, the diameter of the high-strength and high-elongation aluminum alloy rod is 9-10 mm.

9. A high-strength and high-elongation aluminum alloy rod obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the high-strength and high-elongation aluminum alloy rod according to claim 9 in preparing cable monofilaments.

Citation Information

Cited By

  • High-strength high-conductivity heat-resistant aluminum alloy conductor and preparation method thereof

    CN122256765A