A composite positive electrode material layer and its preparation method and application
By using gradient distribution design of 70-90% positive electrode active material and 8-30% sulfide electrolyte in the composite positive electrode material layer of solid-state batteries, the problem that solid-state batteries are difficult to have both high energy density and high power density is solved, and the problem of solid-state batteries is realized Higher electrochemical properties.
Patent Information
- Application Number
- CN202410891481.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-04
AI Technical Summary
Solid-state batteries are difficult to have both high energy density and high power density, and the prior art has kinetic limitations when improving electrochemical performance.
A composite positive electrode material layer is adopted, which contains 70-90% of the positive electrode active material and 8-30% of the sulfide electrolyte, and is distributed in a gradient direction along the thickness direction to ensure the highest mass fraction and lowest mass fraction of the positive electrode active material and the sulfide electrolyte. The difference is between 5% and 30%.
Through the gradient distribution component design, the transmission rate of lithium ions and electrons in the composite positive electrode material layer is improved, and the energy density and power density of solid-state batteries are simultaneously improved.
Smart Images

Figure CN118431406B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy materials, and in particular to a composite positive electrode material layer and a preparation method and application thereof. Background Art
[0002] In order to meet people's demand for high energy density and high safety of energy storage systems, solid-state batteries have shown great application potential in replacing traditional liquid batteries. In solid-state batteries, solid electrolytes are used as diaphragms, and silicon-based negative electrodes or metal lithium negative electrodes with high energy density are used on the negative electrode side. Therefore, the capacity of solid-state batteries is relatively high. In addition, the lack of flammable electrolyte components in solid-state batteries can improve the safety of battery systems.
[0003] At present, the solid electrolytes with the greatest application potential are mainly sulfide electrolytes, oxide electrolytes and halide electrolytes. Among them, sulfide electrolytes are a type of electrolyte material with high ionic conductivity (1-25mS·cm -1 ), so the development of sulfide-based solid-state batteries is the current mainstream development route. Compared with liquid batteries, solid-state batteries still have problems such as low power density, which can be attributed to the kinetic limitations of solid materials. Therefore, the electrochemical performance of solid-state batteries under high surface capacity / high current density conditions needs to be further improved.
[0004] In the composite electrodes of solid-state batteries, the electrolyte and active materials play the role of transporting ions and electrons respectively. However, in thicker electrodes, the ion and electron transport has a larger tortuosity, which limits the transmission rate of electrons and ions. Formula I is the effective electron / ion conductivity:
[0005] (I).
[0006] in, is the effective electronic / ionic conductivity, is the intrinsic electronic / ionic conductivity of the material, is the volume fraction of the material in the electrode, It is the electron / ion transport tortuosity. In addition to the intrinsic electron / ion conductivity of the material, the volume fraction of the material in the composite electrode and the electron / ion transport tortuosity have an impact on the effective electron / ion conductivity in the composite electrode. The volume fraction of the material is usually determined by the feed ratio, while the electron / ion transport tortuosity is related to the uniformity of the distribution of the material in the composite electrode and the porosity.
[0007] In order to further improve the energy density of solid-state batteries, it is usually necessary to prepare electrodes with high areal capacity. However, under high current density (high rate) conditions, the electrochemical performance of solid-state batteries is often limited by electron / ion dynamics, making it impossible to have both high energy density and high power density at the same time. Summary of the invention
[0008] The main purpose of the present invention is to provide a composite positive electrode material layer and a preparation method and application thereof, so as to solve the problem in the prior art that solid-state batteries are difficult to have both high energy density and high power density.
[0009] To achieve the above-mentioned object, according to a first aspect of the present invention, there is provided a composite positive electrode material layer, which comprises the following components in parts by weight: 70-90 parts of positive electrode active material and 8-30 parts of sulfide electrolyte; along the thickness direction of the composite positive electrode material layer, the content of the positive electrode active material and the content of the sulfide electrolyte in the composite positive electrode material are distributed in a gradient manner; along the same thickness direction of the composite positive electrode material layer, the mass fraction of the positive electrode active material decreases from 74%-95% to 60%-85%, and the mass fraction of the sulfide electrolyte increases from 5%-24% to 10%-32%, or, the mass fraction of the positive electrode active material increases from 60%-85% to 74%-95%, and the mass fraction of the sulfide electrolyte decreases from 10%-32% to 5%-24%, and the difference between the highest mass fraction and the lowest mass fraction of each of the positive electrode active material and the sulfide electrolyte is greater than 5% and less than 30%.
[0010] Furthermore, the composite positive electrode material layer further comprises 0-3 parts of a conductive agent and 0.3-4 parts of a binder.
[0011] Furthermore, the conductive agent includes at least one of conductive carbon black, conductive graphite, acetylene black, Ketjen black, carbon nanotubes, vapor-grown carbon fiber, and graphene; and / or the binder includes at least one of styrene-butadiene-styrene triblock copolymer, hydrogenated styrene-butadiene-styrene triblock copolymer, hydrogenated nitrile rubber, nitrile rubber, styrene-ethylene-butylene-styrene copolymer, and fluororubber.
[0012] Furthermore, the weight portion of the positive electrode active material is 75-90 parts, and the weight portion of the sulfide electrolyte is 9-21 parts.
[0013] Furthermore, the positive electrode active material includes at least one of NCM positive electrode material, NCA positive electrode material, LFP positive electrode material, lithium nickel manganese oxide positive electrode material, and lithium-rich manganese-based positive electrode material.
[0014] Furthermore, the sulfide electrolyte includes LPS, Li6PS5X, Li 5.5 PS 4.5 X 1.5 、LiSiPSX、Li 11-a M 2-a P 1+a S 12At least one of, X is selected from at least one of F, Cl, Br, and I, M is selected from at least one of Ge, Si, and Sn, and 0.01≤a≤1.
[0015] Furthermore, the D50 particle size of the positive electrode active material is 0.5-15 μm, and the D50 particle size of the sulfide electrolyte is 0.1-15 μm.
[0016] Furthermore, the positive electrode active material is NCM positive electrode material, and the sulfide electrolyte is Li 5.5 PS 4.5 X 1.5 .
[0017] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned composite positive electrode material layer, the preparation method comprising the following steps:
[0018] S1, dispersing each component in a solvent according to a ratio to obtain a positive electrode slurry;
[0019] S2, coating the positive electrode slurry prepared in S1 onto the surface of the current collector, and drying to obtain a composite positive electrode material layer;
[0020] Among them, in S1, the solid content of the positive electrode slurry is 40%-75%; in S2, the drying conditions are 40-75℃ and 2-40h.
[0021] Furthermore, the solvent is at least one of toluene, xylene, anisole, isobutyl isobutyrate, and butyl butyrate; and / or the coating method is one of blade coating, micro-dimpled coating, slit extrusion coating, spray coating, dip coating, and electrospinning.
[0022] Furthermore, the preparation process of the composite positive electrode material layer is carried out in a dry environment or an inert atmosphere with a dew point below -50°C; and / or the viscosity of the positive electrode slurry is 0.1-0.8 Pa·s.
[0023] In addition, according to the third aspect of the present invention, there is provided an application of the above-mentioned composite positive electrode material layer or the composite positive electrode material layer prepared by the above-mentioned preparation method in a solid-state battery, the solid-state battery comprising a positive electrode current collector, a composite positive electrode material layer, a solid electrolyte layer and a negative electrode pole sheet layer stacked in sequence, a side of the composite positive electrode material layer rich in positive electrode active material is in contact with the positive electrode current collector, and a side of the composite positive electrode material layer rich in sulfide electrolyte is in contact with the solid electrolyte layer.
[0024] By applying the technical solution of the present invention, a composite positive electrode material layer is constructed with positive electrode active materials and sulfide electrolytes, and the usage of the two and the distribution state of the two in the composite positive electrode material layer are limited, the energy density and power density of the solid-state battery can be improved simultaneously. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A schematic diagram of the structure of a solid-state battery prepared from the composite positive electrode material layer of the present invention;
[0026] Figure 2 This is a cross-sectional SEM image of the composite positive electrode material layer of Example 1;
[0027] The above drawings include the following reference numerals:
[0028] 1. Composite positive electrode material layer; 2. Positive electrode current collector; 3. Solid electrolyte layer; 4. Negative electrode layer; 1-1. Positive electrode active material; 1-2. Sulfide electrolyte. DETAILED DESCRIPTION
[0029] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0030] Solid-state batteries are batteries that use solid electrolytes instead of liquid or gel electrolytes. They will not leak or catch fire and generally have a longer service life and higher safety. Solid-state batteries are currently being widely researched and developed and are considered an important part of the next generation of battery technology. They can be used in electric vehicles, mobile devices, and energy storage systems. However, the capacity and power density of solid-state batteries are still far behind those of liquid batteries.
[0031] In order to further improve the electrochemical performance of solid-state batteries, in a typical embodiment of the present invention, a composite positive electrode material layer is provided, which comprises the following components in parts by weight: 70-90 parts of positive electrode active material and 8-30 parts of sulfide electrolyte; along the thickness direction of the composite positive electrode material layer, the content of positive electrode active material and the content of sulfide electrolyte in the composite positive electrode material layer are distributed in a gradient; along the same thickness direction of the composite positive electrode material layer, the mass fraction of the positive electrode active material decreases from 74%-95% to 60%-85%, and the mass fraction of the sulfide electrolyte increases from 5%-24% to 10%-32%, or, the mass fraction of the positive electrode active material increases from 60%-85% to 74%-95%, and the mass fraction of the sulfide electrolyte decreases from 10%-32% to 5%-24%; along the thickness direction of the composite positive electrode material layer, the difference between the highest mass fraction and the lowest mass fraction of the positive electrode active material and the sulfide electrolyte is greater than 5% and less than 30%.
[0032] The positive electrode active material can accept electrons and undergo chemical reactions, which plays a vital role in the capacity of the battery. The electrolyte is used to transmit ions and is a good conductor of ions. Among them, the sulfide electrolyte is a commonly used solid electrolyte material with high ionic conductivity and chemical stability. By selecting the positive electrode active material and the sulfide electrolyte to construct a composite positive electrode material layer, and making the above selections on the amount of the two and the distribution state in the composite positive electrode material layer, both ions and electrons can have good transmission efficiency in the positive electrode material, while increasing the battery energy density and its power density. By limiting the content of the positive electrode active material, the content of the sulfide electrolyte and the gradient of the two along the thickness direction of the composite positive electrode material layer, the transmission rate of lithium ions and electrons in the composite positive electrode material layer can be balanced, thereby further improving the electrochemical performance of the composite positive electrode material layer.
[0033] As a preferred embodiment of the present invention, the composite positive electrode material layer further comprises 0-3 parts of a conductive agent and 0.3-4 parts of a binder. The conductive agent and the binder help improve the conductivity and cycle stability of the battery.
[0034] Typically, but not limiting, the conductive agent includes at least one of conductive carbon black, conductive graphite, acetylene black, Ketjen black, carbon nanotubes, vapor-grown carbon fiber, and graphene; and / or the binder includes at least one of styrene-butadiene-styrene triblock copolymer, hydrogenated styrene-butadiene-styrene triblock copolymer, hydrogenated nitrile rubber, nitrile rubber, styrene-ethylene-butylene-styrene copolymer, and fluororubber.
[0035] As a preferred embodiment of the present invention, the weight portion of the positive electrode active material is 75-90 parts, and the weight portion of the sulfide electrolyte is 9-21 parts.
[0036] The above-mentioned limitation on the amount of positive electrode active material and sulfide electrolyte can make the components in the composite positive electrode material layer have a better gradient distribution state, and greatly improve its power density without losing the battery capacity.
[0037] Typically but not limiting, the positive electrode active material includes at least one of NCM positive electrode material, NCA positive electrode material, LFP positive electrode material, lithium nickel manganese oxide positive electrode material, and lithium-rich manganese-based positive electrode material.
[0038] Typical, but not limiting, sulfide electrolytes include LPS, Li6PS5X, Li 5.5 PS 4.5 X 1.5 、LiSiPSX、Li 11-a M 2-a P 1+a S 12At least one of, X is selected from at least one of F, Cl, Br, I, M is selected from at least one of Ge, Si, Sn, and 0.01≤a≤1; and / or, the D50 particle size of the positive electrode active material is 0.5-15μm, and the D50 particle size of the sulfide electrolyte is 0.1-15μm.
[0039] When the positive electrode active material and the sulfide electrolyte are the above components, the electrochemical performance of the battery is relatively good. In addition, the particle sizes of the positive electrode active material and the sulfide electrolyte are conventional sizes, and they have good comprehensive performance within the above range.
[0040] As a preferred embodiment of the present invention, the positive electrode active material is NCM positive electrode material, and further preferably, the NCM positive electrode material is LiNi 0.9 Co 0.05 Mn 0.05 O2; the above sulfide electrolyte is Li 5.5 PS 4.5 X 1.5 The above-mentioned optimization of the types of the two materials can further improve the capacity of the battery.
[0041] In another typical embodiment of the present invention, a method for preparing the above-mentioned composite positive electrode material layer is provided, and the preparation method comprises the following steps:
[0042] S1, dispersing each component in a solvent according to a ratio to obtain a positive electrode slurry;
[0043] S2, coating the positive electrode slurry prepared in S1 onto the surface of the current collector, and drying to obtain a composite positive electrode material layer;
[0044] Among them, in S1, the solid content of the positive electrode slurry is 40%-75%; in S2, the drying conditions are 40-75℃ and 2-40h.
[0045] The above-mentioned limitations on the solid content and drying conditions of the positive electrode slurry can allow the positive electrode active material and the sulfide electrolyte to migrate as the solvent evaporates. Since the positive electrode active material and the sulfide electrolyte have different densities, the difference between the two is utilized to construct a composite positive electrode material layer with opposite gradient directions of the positive electrode active material and the sulfide electrolyte content. After being assembled into a battery, the end close to the positive electrode current collector is rich in positive electrode active materials, but also contains a certain amount of sulfide electrolyte, while the end close to the electrolyte is rich in sulfide electrolyte and also contains a certain amount of positive electrode active materials, thereby enabling the battery to have good energy density and power density.
[0046] Typically, but not limiting, the solvent is at least one of toluene, xylene, anisole, isobutyl isobutyrate, butyl butyrate; and / or the coating method is one of blade coating, micro-dimple coating, slot extrusion coating, spray coating, dip coating, and electrospinning.
[0047] As a preferred embodiment of the present invention, the preparation process of the composite positive electrode material layer is carried out in a dry environment or inert atmosphere with a dew point below -50° C. Preparation under the above conditions can avoid the introduction of other impurities.
[0048] As a preferred embodiment of the present invention, the viscosity of the positive electrode slurry is 0.1-0.8 Pa·s. The above-mentioned limitation on the viscosity of the positive electrode slurry can form a good gradient of the content of the positive electrode active material and the sulfide electrolyte in the composite positive electrode material layer, thereby increasing the transmission rate of ions and electrons in the composite positive electrode material layer. In the description of the present invention, the viscosity is measured at 25°C using a rheometer.
[0049] In another typical embodiment of the present invention, there is provided an application of the above-mentioned composite positive electrode material layer or the composite positive electrode material layer prepared by the above-mentioned preparation method in a solid-state battery, the solid-state battery comprising a positive electrode current collector, a composite positive electrode material layer, a solid electrolyte layer and a negative electrode pole layer stacked in sequence, a side of the composite positive electrode material layer rich in positive electrode active material is in contact with the positive electrode current collector, and a side of the composite positive electrode material layer rich in sulfide electrolyte is in contact with the solid electrolyte layer.
[0050] The “side rich in positive electrode active materials” mentioned in the present application represents the side having the highest content of positive electrode active materials along the thickness direction of the composite positive electrode material layer, and the “side rich in sulfide electrolyte” represents the side having the highest content of sulfide electrolyte along the thickness direction of the composite positive electrode material layer.
[0051] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0052] The materials used in the embodiments and comparative examples are as follows:
[0053] Positive electrode active material: LiNi 0.8 Co 0.1 Mn 0.1 O2, D50 particle size is 4 μm; LiNi 0.9 Co 0.05 Mn 0.05 O2, D50 particle size is 4 μm;
[0054] Sulfide electrolyte: Li6PS5Cl, D50 particle size 3 μm; Li 5.5 PS 4.5 Cl1.5 , D50 particle size is 3 μm;
[0055] Binder: styrene-butadiene-styrene triblock copolymer;
[0056] Solvent: isobutyl isobutyrate;
[0057] Foil material: Al foil, 20 μm.
[0058] The composite positive electrode material layers in the examples and comparative examples were prepared in a drying room with a dew point below -50°C.
[0059] Examples 1-10
[0060] The embodiment of the composite positive electrode material layer of the present invention is prepared as follows:
[0061] S1, dispersing each component in isobutyl isobutyrate according to a ratio to obtain a positive electrode slurry;
[0062] S2, the positive electrode slurry was coated on the surface of the foil by blade coating and dried in a blast oven to obtain a surface capacity of 5 mAh cm -2 A composite positive electrode material layer and a positive electrode sheet;
[0063] Comparative Example 1
[0064] A composite positive electrode material layer, the composite positive electrode material layer is different from that of Example 3 in that the contents of sulfide electrolyte and binder are different, as specifically shown in Table 1.
[0065] Comparative Example 2
[0066] A composite positive electrode material layer, the difference between the composite positive electrode material layer and Example 1 is that the solid content and drying conditions of the positive electrode slurry are different, as shown in Table 1.
[0067] The components of the composite positive electrode material layer, their amounts (parts by weight) and preparation conditions are shown in Table 1.
[0068] Table 1
[0069]
[0070] Performance Test:
[0071] 1. The mass fraction of the positive electrode active material (A1) and the mass fraction of the sulfide electrolyte (A2) on the side rich in the positive electrode active material in the composite positive electrode material layer, as well as the mass fraction of the positive electrode active material (E1) and the mass fraction of the sulfide electrolyte (E2) on the side rich in the sulfide electrolyte were tested and calculated by an energy spectrometer. The test results are shown in Table 2.
[0072] 2. The positive electrode sheet prepared by the composite positive electrode material layer of the embodiment and the comparative example is combined with Li 0.5 In negative electrode was assembled into half-cell for rate performance test, in which the sulfide electrolyte-rich side was connected with Li 0.5 In negative electrode is connected, and the test results are shown in Table 3.
[0073] Table 2
[0074]
[0075] Table 3
[0076]
[0077] As shown in Table 3, the discharge capacity of the composite positive electrode material layers prepared in Examples 1-10 under 0.05C conditions can reach 190 mAh·g -1 Above, the 1C capacity can reach 95 mAh g -1 The results show that compared with the positive electrode material layer with uniform distribution of components, the positive electrode material layer with gradient distribution of positive electrode active material and electrolyte has relatively better electrochemical performance, and the power density of the battery made therefrom is higher.
[0078] In addition, by comparing the test results of Examples 3-7, it can be found that when the weight parts of the positive electrode active material are 75-90 parts and the weight parts of the sulfide electrolyte are 9-21 parts, the 1C / 0.05C capacity ratio is higher than 50%, and has good energy density and power density.
[0079] By comparing the test results of Examples 8-9 and Example 3, it can be found that when the positive electrode active material is NCM positive electrode material and LiNi 0.9 Co 0.05 Mn 0.05 O2, the discharge capacity and rate performance of the battery are significantly better; in addition, the sulfide electrolyte is Li 5.5 PS 4.5 X 1.5 Its electrochemical performance is better.
[0080] By comparing the test results of Examples 3-5 and Example 10, it can be found that when the amount of the binder is 0.3-4 parts, the rate performance is better.
[0081] Figure 1 The structure diagram of the solid-state battery prepared by the composite positive electrode material layer of the present invention; wherein: 1, composite positive electrode material layer; 2, positive electrode current collector; 3, solid electrolyte layer; 4, negative electrode sheet layer; 1-1, positive electrode active material; 1-2, sulfide electrolyte; Figure 2 This is a cross-sectional SEM image of the composite positive electrode material layer of Example 1; wherein: 1-1, positive electrode active material; 1-2, sulfide electrolyte. As can be seen from the figure, the positive electrode active material and sulfide electrolyte in the composite positive electrode material layer are distributed in a gradient, and the gradient directions of the two are opposite. The above solid-state battery has a high energy density (≥5mAh·cm -2 ) and good power density.
[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composite positive electrode material layer, characterized in that: The invention comprises the following components in parts by weight: 75-90 parts of positive electrode active material and 9-21 parts of sulfide electrolyte; along the thickness direction of the composite positive electrode material layer, the content of the positive electrode active material and the content of the sulfide electrolyte are distributed in a gradient; along the same thickness direction of the composite positive electrode material layer, the mass fraction of the positive electrode active material decreases from 74%-95% to 60%-85%, and the mass fraction of the sulfide electrolyte increases from 5%-24% to 10%-32%, or, the mass fraction of the positive electrode active material increases from 60%-85% to 74%-95%, and the mass fraction of the sulfide electrolyte decreases from 10%-32% to 5%-24%, and the difference between the highest mass fraction and the lowest mass fraction of each of the positive electrode active material and the sulfide electrolyte is greater than or equal to 6% and less than or equal to 27%; The positive electrode active material includes LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.9 Co 0.05 Mn 0.05 O2, the sulfide electrolyte includes Li6PS5X, Li 5.5 PS 4.5 X 1.5 At least one of, X is selected from at least one of F, Cl, Br, and I.
2. The composite positive electrode material layer according to claim 1, characterized in that: It also contains 0-3 parts of conductive agent and 0.3-4 parts of binder.
3. The composite positive electrode material layer according to claim 2, characterized in that: The conductive agent comprises at least one of conductive carbon black, conductive graphite, acetylene black, Ketjen black, carbon nanotubes, vapor-grown carbon fiber, and graphene; and / or the binder comprises at least one of styrene-butadiene-styrene triblock copolymer, hydrogenated styrene-butadiene-styrene triblock copolymer, hydrogenated nitrile rubber, nitrile rubber, styrene-ethylene-butylene-styrene copolymer, and fluororubber.
4. The composite positive electrode material layer according to any one of claims 1 to 3, characterized in that: The D50 particle size of the positive electrode active material is 0.5-15 μm, and the D50 particle size of the sulfide electrolyte is 0.1-15 μm.
5. The composite positive electrode material layer according to claim 4, characterized in that: The sulfide electrolyte is Li 5.5 PS 4.5 X 1.5 .
6. A method for preparing a composite positive electrode material layer according to any one of claims 1 to 5, characterized in that: The steps include: S1, dispersing each component in a solvent according to a ratio to obtain a positive electrode slurry; S2, coating the positive electrode slurry onto the surface of the current collector and drying to obtain the composite positive electrode material layer; In S1, the solid content of the positive electrode slurry is 40%-75%; in S2, the drying conditions are 40-75° C. and 2-40 hours.
7. The preparation method according to claim 6, characterized in that: The solvent is at least one of toluene, xylene, anisole, isobutyl isobutyrate and butyl butyrate; and / or, The coating is one of blade coating, micro-dimple coating, slit extrusion coating, spray coating, dip coating, and electrostatic spinning.
8. The preparation method according to claim 6 or 7, characterized in that: The preparation process of the composite positive electrode material layer is carried out in a dry environment or an inert atmosphere with a dew point below -50°C; and / or the viscosity of the positive electrode slurry is 0.1-0.8 Pa·s.
9. Use of the composite positive electrode material layer according to any one of claims 1 to 5 or the composite positive electrode material layer prepared by the preparation method according to any one of claims 6 to 8 in a solid-state battery, characterized in that: The solid-state battery includes a positive electrode current collector, a composite positive electrode material layer, a solid electrolyte layer and a negative electrode plate layer which are stacked in sequence, wherein a side of the composite positive electrode material layer rich in the positive electrode active material is in contact with the positive electrode current collector, and a side of the composite positive electrode material layer rich in the sulfide electrolyte is in contact with the solid electrolyte layer.
Citation Information
Patent Citations
Preparation method of high-nickel ternary positive pole piece and preparation method of sulfide solid-state battery
CN114824174A