Polyurethane forklift wheel material with strong environmental adaptability and preparation method thereof
Through the combination of block copolymerized polyols with MDI-type low-free prepolymers and nanometal oxides, the stability of polyurethane forklift wheels under temperature and humidity changes is solved, and high strength, low endogenous heat and Good environmental adaptability results extend service life and improve performance.
Patent Information
- Application Number
- CN202410873578.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-02
AI Technical Summary
The existing polyurethane forklift wheels are facing defects and damage caused by large temperature changes, humidity changes and continuous use, and it is difficult to meet the needs of high strength, low endogenous heat and environmental adaptability.
The block copolymerized polyol is combined with MDI type low-free prepolymer and is equipped with nanometal oxides. Through scientific and reasonable formulation design, the thermal conductivity and durability of polyurethane forklift wheel materials are improved, and its rebound performance and resistance are improved. Tear.
It realizes high strength, low endogenous heat and good environmental adaptability of polyurethane forklift wheel materials, extends service life and meets high performance needs at different temperatures.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane elastomers, and in particular relates to a polyurethane forklift wheel material with strong environmental adaptability and a preparation method thereof. Background Art
[0002] As one of the basic parts of forklifts and the main component of forklift power transmission, forklift wheels directly affect the forklift's energy consumption, safety, service life, operability and temperature adaptability. As one of the forklift wheel series, polyurethane forklift wheels must not only show the wear resistance, tear resistance and long life characteristics common to conventional rubber tires and other composite tires in practical applications, but also have the ability to resist the impact of various external environments on tires. It must maintain excellent rebound performance, reduce endogenous heat, and have excellent corrosion resistance. Therefore, polyurethane forklift wheels have been more widely used. As a special material product, it can still show excellent performance in different application environments, becoming an excellent choice in the field of forklift wheels.
[0003] Conventional polyurethane forklift wheels are mainly divided into two categories: polyester and PTMG. Polyester forklift wheels have higher hardness, tear strength and wear resistance due to the presence of internal ester bonds, but they also have poor elasticity and high friction endogenous heat. The rubber coating is hard and brittle and easy to break at low temperatures, the starting force is increased, and it is not resistant to hydrolysis; PTMG forklift wheels have higher flexibility in ether bonds, which makes it have higher resilience and lower endogenous heat friction in external performance. Therefore, in low-temperature use scenarios, ether bonds show better performance. However, the strength of the ether bond itself is low, which makes the hardness and tear strength of the product much lower than that of polyester products with the same content, and the load-bearing capacity of the caster is seriously reduced during high temperatures in summer. In view of the concern about the safety and service life of forklift tires, considering the large temperature changes, high humidity, severe performance degradation, and defects caused by continuous use in the use environment of forklift wheels, such as explosion, degumming, reduced load-bearing capacity, and increased static pressure, it is necessary to prepare a polyurethane forklift wheel material that not only has excellent mechanical strength and environmental adaptability, but also has low endogenous heat and can meet market demand. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a polyurethane forklift wheel material with strong environmental adaptability, which combines the advantages of polyester and polyether and exhibits excellent strength, tear resistance and elasticity; at the same time, by adding nano metal oxides to the formula components, the thermal conductivity of the polyurethane forklift wheel material is improved, the endogenous heat is reduced, and its durability is improved;
[0005] Another object of the present invention is to provide a method for preparing a polyurethane forklift wheel material with strong environmental adaptability, which is scientific, reasonable, simple and easy to implement.
[0006] The technical solution adopted by the present invention is as follows:
[0007] The polyurethane forklift wheel material with strong environmental adaptability comprises a curing agent component and a prepolymer component in a mass ratio of (39.5-44.4):100;
[0008] The curing agent component is made of the following raw materials in parts by weight:
[0009] 1.25-2.5 parts of small molecule polyols;
[0010] 7.5-28.25 parts of difunctional secondary amine p-phenylenediamine curing agent;
[0011] 12.5-35 parts of block copolymer polyol;
[0012] Catalyst 0.25-1.12 parts;
[0013] The prepolymer component is 100 parts by mass of block copolymer polyol-MDI type low free prepolymer;
[0014] The preparation method of the block copolymer polyol-MDI type low-free prepolymer is as follows: the block copolymer polyol and MDI type isocyanate with a mass ratio of (37.5-50.75): (49.25-62.5) are added into a reactor respectively, and the reaction is carried out by heat preservation, and then nano metal oxide is added and continued to be stirred, and vacuum degassing is performed to obtain the block copolymer polyol-MDI type low-free prepolymer; the amount of the nano metal oxide used is (0.1-1) wt.% of the total amount of the prepolymer components.
[0015] The small molecule polyol is one of 1,4-butanediol, trimethylolpropane, triethanolamine or ethylene glycol.
[0016] The bifunctional secondary amine p-phenylenediamine curing agent is one or more of absintheine, N,N-diisopropyl p-phenylenediamine, N,N'-di-sec-butyl p-phenylenediamine, 4,4-methylenebis(N-methylaniline) or 4,4'-bis-sec-butylaminodiphenylmethane.
[0017] The block copolymer polyol is one or more of Capa 7201A (PCL and PTMG copolymer polyol, hydroxyl value 56 mg KOH / g, functionality 2), Capa 8015D (PCL and PLA copolymer polyol, hydroxyl value 112 mg KOH / g, functionality 2), Capa8025D (PCL and PLA copolymer polyol, hydroxyl value 56 mg KOH / g, functionality 2), Capa 8025E (PCL and PLA copolymer polyol, hydroxyl value 56 mg KOH / g, functionality 3) or Capa 7203 (PCL and PC copolymer polyol, hydroxyl value 56 mg KOH / g, functionality 2).
[0018] The catalyst is one of DXD-06C, DXD-07C or CH-05.
[0019] The nano metal oxide is one of nano zinc oxide, nano aluminum oxide or nano magnesium oxide, and the particle size is 20-50nm.
[0020] The MDI type isocyanate is one or more of carbodiimide modified diphenylmethane diisocyanate (liquefied MDI), polymethylene polyphenyl polyisocyanate (polymeric MDI), MDI-100 or MDI-50.
[0021] The polyurethane forklift wheel material with strong environmental adaptability has a room temperature hardness of ≥94A / 48D, a room temperature rebound rate of ≥50%, a low temperature rebound rate of ≥40%, and a right-angle tear strength of >120kN / m.
[0022] The method for preparing the polyurethane forklift wheel material with strong environmental adaptability comprises the following steps:
[0023] (1) Putting a small molecule polyol and a block copolymer polyol into a reaction kettle, vacuum dehydrating to a water content of ≤0.05wt.%, cooling to below 60°C, adding a difunctional secondary amine p-phenylenediamine type curing agent and a catalyst, and mixing evenly to obtain a curing agent component;
[0024] (2) Add block copolymer polyol and MDI isocyanate in a mass ratio of (37.5-50.75): (49.25-62.5) into a reactor, respectively, and heat-retain the reaction at 75-85°C for 2.5-3h, then add nano-metal oxide and continue stirring for 30min, and remove bubbles under vacuum ≤-0.095MPa to obtain a block copolymer polyol-MDI low-free prepolymer; its -NCO content is (13-19)wt.%;
[0025] (3) The curing agent component and the prepolymer component are kept warm at 60-65°C and 75-80°C respectively. When in use, the curing agent component and the prepolymer component are evenly mixed in a mass ratio of (39.5-44.4):100, poured into a mold at 101-110°C, and post-vulcanized at a temperature of 100-105°C for 16-20h after the mold is opened to obtain a polyurethane forklift wheel material with strong environmental adaptability.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The environmentally adaptable polyurethane forklift wheel material described in the present invention uses unconventional block copolymer polyols. This material combines the dual characteristics of polyester and polyether polyurethane at the molecular chain level. Compared with simple polyester, polyether, polycaprolactone or their physical blends, it exhibits more excellent performance. It is matched with a bifunctional secondary amine p-phenylenediamine curing agent to further improve the rebound performance and strength of the product. In order to further enhance the durability of the forklift wheel, an appropriate amount of nano-metal oxide is added to the prepolymer component, which significantly improves the thermal conductivity of the tire and reduces the accumulation of internal heat, thereby effectively extending the service life of the tire;
[0028] (2) Through careful formula design, the polyurethane forklift wheel material with strong environmental adaptability described in the present invention has rebound and tear resistance properties that meet and exceed the industry requirements, including hardness of 96A / 48D-98A / 55D, right-angle tear strength>120kN / m, normal temperature rebound rate ≥50%, low temperature rebound rate ≥40%, and a wide range that can meet the production needs of different manufacturers. The forklift wheel product made of the polyurethane forklift wheel material with strong environmental adaptability has a minimum running temperature of only 70°C, and the overall performance is far superior to the existing polyurethane forklift wheel products;
[0029] (3) The method for preparing the polyurethane forklift wheel material with strong environmental adaptability described in the present invention is scientific, reasonable, simple and easy to implement. DETAILED DESCRIPTION
[0030] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.
[0031] Unless otherwise specified, the raw materials used in the examples and comparative examples are conventional commercially available raw materials, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.
[0032] Some of the raw materials used in the examples and comparative examples are described as follows:
[0033] Absintheine was purchased from Shanghai Qiam Analytical Technology Co., Ltd.;
[0034] N,N-diisopropyl-p-phenylenediamine was purchased from Hangzhou Dayang Chemical Co., Ltd.;
[0035] N,N'-di-sec-butyl-p-phenylenediamine was purchased from Tianmen Hengchang Chemical Co., Ltd.;
[0036] 4,4-Methylenebis(N-methylaniline) was purchased from Wuhan Shiruikai Technology Co., Ltd.;
[0037] 4,4'-bis-sec-butylaminodiphenylmethane was purchased from Yantai Wanhua Polyurethane Co., Ltd.;
[0038] Capa 7201A, purchased from Ingevity, USA;
[0039] Capa 8015D, purchased from Ingevity, USA;
[0040] Capa 8025D, purchased from Ingevity, USA;
[0041] Capa 8025E, purchased from Ingevity, USA;
[0042] Capa 7203, purchased from Ingevity, USA;
[0043] DXD-06C, purchased from Shandong Yinuowei Polyurethane Co., Ltd.;
[0044] DXD-07C, purchased from Shandong Yinuowei Polyurethane Co., Ltd.;
[0045] CH-05, purchased from Guangzhou Yourun Synthetic Materials Co., Ltd.;
[0046] Nano magnesium oxide DK-MgO-001, purchased from Beijing Dekedaojin Technology Co., Ltd., with a particle size of 25 ± 5 nm;
[0047] Nano magnesium oxide ZT-Mg30, purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd.; particle size 40 ± 10 nm;
[0048] Nano-alumina ZT-L30M, purchased from Zhejiang Zhitai Nano-Micro New Materials Co., Ltd.; particle size 30 nm;
[0049] Nano zinc oxide ZT-J20, purchased from Zhejiang Zhiti Nano Micro New Materials Co., Ltd.; particle size 20 nm;
[0050] Nano zinc oxide ZT-J50, purchased from Zhejiang Zhitai Nano Micro New Materials Co., Ltd.; particle size 50 nm;
[0051] PCL2202T, purchased from Juren Chemical New Materials Technology Co., Ltd.;
[0052] PTMG2000 was purchased from BASF AG, Germany.
[0053] Example 1
[0054] The polyurethane forklift wheel material with strong environmental adaptability comprises a curing agent component and a prepolymer component in a mass ratio of 42.87:100;
[0055] The curing agent component is made of the following raw materials in parts by weight:
[0056] 1,4-Butanediol: 1.25 parts;
[0057] Absintheine: 28.25 parts;
[0058] Capa 8015D: 12.5 parts;
[0059] DXD-07C: 0.87 parts;
[0060] The prepolymer component is 100 parts by mass of block copolymer polyol-MDI type low free prepolymer;
[0061] The method for preparing the polyurethane forklift wheel material with strong environmental adaptability comprises the following steps:
[0062] (1) 1,4-Butanediol and Capa 8015D were placed in a reaction kettle, vacuum dehydrated to a water content of 0.03 wt.%, cooled to 60°C, and absintheline and DXD-07C were added and mixed evenly to obtain a curing agent component;
[0063] (2) 50.75 parts of Capa 7201A were added to the reactor, and then 34.47 parts of MDI-100 and 14.78 parts of liquefied MDI were mixed evenly and slowly added to the reactor. The mixture was kept warm at 75°C for 3 hours, and then ZT-Mg30 was added and stirred for 30 minutes. The bubbles were removed under vacuum conditions of -0.095 MPa to obtain a block copolymer polyol-MDI type low free prepolymer; the -NCO content of the prepolymer was 13.6wt.%; the amount of ZT-Mg30 was 1wt.% of the total amount of the prepolymer components;
[0064] (3) The curing agent component and the prepolymer component are kept warm at 64°C and 80°C respectively. When in use, the curing agent component and the prepolymer component are mixed evenly and poured into a mold at 105°C. After the mold is opened, post-vulcanization is performed at a temperature of 103°C for 19 hours to obtain a polyurethane forklift wheel material with strong environmental adaptability.
[0065] Example 2
[0066] The polyurethane forklift wheel material with strong environmental adaptability comprises a curing agent component and a prepolymer component in a mass ratio of 39.5:100;
[0067] The curing agent component is made of the following raw materials in parts by weight:
[0068] 1,4-Butanediol: 2.5 parts;
[0069] N,N-diisopropyl-p-phenylenediamine: 6.25 parts;
[0070] 4,4-Methylenebis(N-methylaniline): 10 parts;
[0071] Capa 8015D: 20 copies;
[0072] CH-05: 0.75 parts;
[0073] The prepolymer component is 100 parts by mass of block copolymer polyol-MDI type low free prepolymer;
[0074] The method for preparing the polyurethane forklift wheel material with strong environmental adaptability comprises the following steps:
[0075] (1) 1,4-Butanediol and Capa 8015D were placed in a reaction kettle, vacuum dehydrated to a water content of 0.04wt.%, cooled to 55°C, N,N-diisopropyl-p-phenylenediamine, 4,4-methylenebis(N-methylaniline) and CH-05 were added, and mixed evenly to obtain a curing agent component;
[0076] (2) 47.5 parts of Capa 8025D were added to the reactor, and then 26.25 parts of polymerized MDI and 26.25 parts of MDI-50 were mixed evenly and then slowly added to the reactor. The mixture was kept warm at 77°C for 3 hours, and then ZT-J50 was added and stirred for 30 minutes. The bubbles were removed under vacuum conditions of -0.095 MPa to obtain a block copolymer polyol-MDI type low free prepolymer; the -NCO content of the prepolymer was 14.6wt.%; the amount of ZT-J50 was 0.8wt.% of the total amount of the prepolymer components;
[0077] (3) The curing agent component and the prepolymer component are kept warm at 62°C and 75°C respectively. When in use, the curing agent component and the prepolymer component are mixed evenly and poured into a mold at 101°C. After the mold is opened, post-vulcanization is performed at 100°C for 18 hours to obtain a polyurethane forklift wheel material with strong environmental adaptability.
[0078] Example 3
[0079] The polyurethane forklift wheel material with strong environmental adaptability comprises a curing agent component and a prepolymer component in a mass ratio of 42.75:100;
[0080] The curing agent component is made of the following raw materials in parts by weight:
[0081] Triethanolamine: 1.87 parts;
[0082] N,N'-di-sec-butyl-p-phenylenediamine: 6.88 parts;
[0083] 4,4'-bis-sec-butylaminodiphenylmethane: 7.5 parts;
[0084] Capa 7201A: 26.25 copies;
[0085] DXD-06C: 0.25 parts;
[0086] The prepolymer component is 100 parts by mass of block copolymer polyol-MDI type low free prepolymer;
[0087] The method for preparing the polyurethane forklift wheel material with strong environmental adaptability comprises the following steps:
[0088] (1) Triethanolamine and Capa 7201A were placed in a reaction kettle, vacuum dehydrated to a water content of 0.05 wt.%, cooled to 55°C, N,N'-di-sec-butyl-p-phenylenediamine, 4,4'-di-sec-butylaminodiphenylmethane and DXD-06C were added, and mixed evenly to obtain a curing agent component;
[0089] (2) 11.25 parts of Capa 7203 and 26.25 parts of Capa 8025D were added to the reactor, and then 6.25 parts of polymerized MDI and 56.25 g of MDI-100 were mixed evenly and slowly added to the reactor. The mixture was kept warm at 80°C for 3 hours, and then ZT-J20 was added and stirred for 30 minutes. The bubbles were removed under vacuum conditions of -0.095 MPa to obtain a block copolymer polyol-MDI type low free prepolymer; the -NCO content of the prepolymer was 19 wt.%; the amount of ZT-J20 used was 0.5 wt.% of the total amount of the prepolymer components;
[0090] (3) The curing agent component and the prepolymer component are kept warm at 63°C and 78°C respectively. When in use, the curing agent component and the prepolymer component are mixed evenly and poured into a mold at 107°C. After the mold is opened, post-vulcanization is performed at a temperature of 105°C for 20 hours to obtain a polyurethane forklift wheel material with strong environmental adaptability.
[0091] Example 4
[0092] The polyurethane forklift wheel material with strong environmental adaptability comprises a curing agent component and a prepolymer component in a mass ratio of 43.62:100;
[0093] The curing agent component is made of the following raw materials in parts by weight:
[0094] Trihydroxypropane: 1.25 parts;
[0095] Absintheine: 5 parts;
[0096] 4,4'-bis-sec-butylaminodiphenylmethane: 6.25 parts;
[0097] Capa 7203: 15 copies;
[0098] Capa 8025D: 15 parts;
[0099] DXD-07C: 1.12 parts;
[0100] The prepolymer component is 100 parts by mass of block copolymer polyol-MDI type low free prepolymer;
[0101] The method for preparing the polyurethane forklift wheel material with strong environmental adaptability comprises the following steps:
[0102] (1) Trihydroxypropane, Capa 7203 and Capa 8025D are placed in a reaction kettle, vacuum dehydrated to a water content of 0.02 wt.%, cooled to 60°C, and absintheline, 4,4'-bis-sec-butylaminodiphenylmethane and DXD-07C are added, and mixed evenly to obtain a curing agent component;
[0103] (2) 3.75 parts of Capa 8025E and 40 parts of Capa 8025D were added to the reactor, and then 6.25 parts of MDI-50, 12.5 parts of liquefied MDI and 37.5 parts of MDI-100 were mixed evenly and slowly added to the reactor. The mixture was kept warm at 82°C for 3 hours, and then ZT-L30M was added and stirred for 30 minutes. The bubbles were removed under vacuum conditions of -0.095 MPa to obtain a block copolymer polyol-MDI type low free prepolymer; the -NCO content of the prepolymer was 16.3wt.%; the amount of ZT-L30M was 0.3wt.% of the total amount of the prepolymer components;
[0104] (3) The curing agent component and the prepolymer component are kept warm at 65°C and 80°C respectively. When in use, the curing agent component and the prepolymer component are mixed evenly and poured into a mold at 110°C. After the mold is opened, post-vulcanization is performed at 100°C for 16 hours to obtain a polyurethane forklift wheel material with strong environmental adaptability.
[0105] Example 5
[0106] The polyurethane forklift wheel material with strong environmental adaptability comprises a curing agent component and a prepolymer component in a mass ratio of 44.4:100;
[0107] The curing agent component is made of the following raw materials in parts by weight:
[0108] Ethylene glycol: 1.25 parts;
[0109] N,N'-di-sec-butyl-p-phenylenediamine: 5 parts;
[0110] 4,4-methylenebis(N-methylaniline): 2.5 parts;
[0111] Capa 8015D: 22.5 parts;
[0112] Capa 8025E: 12.5 parts;
[0113] CH-05: 0.65 parts;
[0114] The prepolymer component is 100 parts by mass of block copolymer polyol-MDI type low free prepolymer;
[0115] The method for preparing the polyurethane forklift wheel material with strong environmental adaptability comprises the following steps:
[0116] (1) Ethylene glycol, Capa 8015D and Capa 8025E were placed in a reaction kettle, vacuum dehydrated to a water content of 0.03wt.%, cooled to 55°C, N,N'-di-sec-butyl-p-phenylenediamine, 4,4-methylenebis(N-methylaniline) and CH-05 were added, and mixed evenly to obtain a curing agent component;
[0117] (2) 20 parts of Capa 8025D and 30 parts of Capa 7201A were added to the reactor, and then 5 parts of polymerized MDI, 15 parts of liquefied MDI and 30 parts of MDI-100 were mixed evenly and slowly added to the reactor. The mixture was kept warm at 85°C for 2.5 hours, and then DK-MgO-001 was added and stirred for 30 minutes. The bubbles were removed under vacuum conditions of -0.095 MPa to obtain a block copolymer polyol-MDI type low-free prepolymer; the -NCO content of the prepolymer was 13.7wt.%; the amount of DK-MgO-001 was 0.1wt.% of the total amount of the prepolymer components;
[0118] (3) The curing agent component and the prepolymer component are kept warm at 60°C and 75°C respectively. When in use, the curing agent component and the prepolymer component are mixed evenly and poured into a mold at 105°C. After the mold is opened, post-vulcanization is performed at 100°C for 16 hours to obtain a polyurethane forklift wheel material with strong environmental adaptability.
[0119] Comparative Example 1
[0120] The difference from Example 1 is that the block copolymer polyol in the curing agent component is replaced by a mixture of PCL2202T and PTMG2000 having the same relative molecular mass as Capa8015D, the mass ratio of PCL2202T to PTMG2000 is 1:1, the initiator of PCL2202T is 1,4-butanediol, and the rest is the same as Example 1.
[0121] Comparative Example 2
[0122] The difference from Example 3 is that when preparing the block copolymer polyol-MDI type low free prepolymer, no nano metal oxide is added, and the rest is the same as Example 3.
[0123] Comparative Example 3
[0124] The difference from Example 2 is that the difunctional secondary amine p-phenylenediamine curing agent in the curing agent component is replaced with an equal amount of triethanolamine, and the rest is the same as Example 2.
[0125] Comparative Example 4
[0126] The difference from Example 4 is that the trihydroxypropane in the curing agent component is replaced with 0.25 parts of trihydroxypropane, 0.5 parts of absinthe and 0.5 parts of 4,4'-bis-sec-butylaminodiphenylmethane, and the rest is the same as Example 4.
[0127] Comparative Example 5
[0128] The difference from Example 5 is that the preparation method of the prepolymer component is: 26.2 parts of Capa 8025D and 39.3 parts of Capa 7201A are added to a reactor, and then 34.5 parts of TDI-100 are mixed evenly and slowly added to the reactor, and the mixture is kept warm at 85°C for 2.5 hours, and then DK-MgO-001 is added and stirred for 30 minutes, and bubbles are removed under vacuum conditions of -0.095MPa to obtain a block copolymer polyol-MDI type low free prepolymer; the -NCO content thereof is 13.7wt.%; and the rest is the same as Example 5.
[0129] The polyurethane forklift wheel materials prepared in Examples 1-5 and Comparative Examples 1-5 were subjected to performance tests, and the test method was as follows:
[0130] Room temperature hardness (Shore A / Shore D): refer to GB / T 531.1-2008;
[0131] Normal temperature rebound rate (%, 25℃): refer to GB / T 1681-2009;
[0132] Right-angle tear strength (kN / m): refer to GB / T 529-2008;
[0133] Low temperature rebound rate (%, 0℃): refer to GB / T 1681-2009;
[0134] Running test temperature (°C): Forklift wheel products prepared by using the polyurethane forklift wheel materials of Examples 1-5 and Comparative Examples 1-5 were respectively mounted on a crawler trolley with a load of 700 kg. The trolley was allowed to test at a speed of 4 km / h on a flat surface. The temperature rise of the forklift wheel products was measured in real time, and the temperature after long-term operation and stabilization was observed to determine the dynamic endogenous heat performance of the tire.
[0135] The test results are shown in Table 1:
[0136] Table 1 Performance test results
[0137]
[0138] From the data in Table 1, it can be seen that the room temperature hardness of the polyurethane forklift wheel materials prepared in Examples 1-5 is ≥94A / 48D, the room temperature rebound rate is ≥50%, the low temperature rebound rate is also ≥40%, the right-angle tear strength is >120kN / m, and all indicators are excellent;
[0139] It can be seen from Examples 1-5 and Comparative Example 2 that the nano metal oxide added to the prepolymer component has a very obvious effect on the temperature rise of the forklift wheel product, and its addition amount has a direct negative correlation trend with the temperature rise, indicating that the addition of nano metal oxide can effectively reduce endogenous heat and increase the heat extraction rate.
[0140] By comparing Example 1 and Comparative Example 1, it can be seen that due to the use of Capa series block copolymer polyols, the mechanical properties are significantly better than those of traditional polycaprolactone and PTMG components. Compared with the physical mixture of polycaprolactone and PTMG polyether, the internal chain segments of the block copolymer polyols are more functional, with both caprolactone-type segments providing strength and polyether-type segments providing flexibility and elasticity. Therefore, although the hardness of the product is slightly reduced, its tear strength is higher than that of the caprolactone type, and its room temperature and low temperature rebound are also higher than those of the physically mixed PTMG-caprolactone type products.
[0141] By comparing Example 2 and Comparative Example 3, it can be seen that the difunctional secondary amine p-phenylenediamine curing agent in the curing agent component has a unique benzene ring hyperconjugated structure, that is, the P-π conjugated form itself can form a relatively wide electron cloud, thereby significantly improving the bonding ability. The good conjugated structure also makes its overall structure more regular and orderly, thereby making the product more flexible and ductile, and it is easier to form a regular crystalline structure between the chain segments, thereby improving the rebound performance; and due to the wide distribution of its electron cloud, its intermolecular force is also stronger, and the tear resistance is also improved.
[0142] Comparison of Example 4 with Comparative Example 4 shows that the small molecule polyol in the curing agent component also plays an important role in improving the hardness of the product and improving the tear strength. Without adding the small molecule polyol, the hardness and tear strength are significantly reduced, so it is necessary to add a certain amount of small molecule alcohol to balance the performance of the curing agent.
[0143] Comparing Example 5 with Comparative Example 5, after replacing MDI type isocyanate with TDI type isocyanate, its hardness tear strength is improved, but the rebound and running resistance performance are significantly reduced. The reason is that TDI has a stronger molecular chain rigidity than MDI, which is manifested in a higher hardness tear strength. The MDI type bisphenylcycloalkyl has better configuration mobility and lower molecular tension, which is manifested in better elasticity and better running resistance.
Claims
1. A polyurethane forklift wheel material with strong environmental adaptability, characterized in that: It includes a curing agent component and a prepolymer component in a mass ratio of (39.5-44.4):100; The curing agent component is made of the following raw materials in parts by weight: 1.25-2.5 parts of small molecule polyols; 7.5-28.25 parts of difunctional secondary amine p-phenylenediamine curing agent; 12.5-35 parts of block copolymer polyol; Catalyst 0.25-1.12 parts; The prepolymer component is 100 parts by mass of block copolymer polyol-MDI type low free prepolymer; The preparation method of the block copolymer polyol-MDI type low free prepolymer is as follows: the block copolymer polyol and MDI type isocyanate with a mass ratio of (37.5-50.75): (49.25-62.5) are added to a reactor respectively, and the reaction is carried out by heat preservation, and then nano metal oxide is added and continued to be stirred, and vacuum degassing is performed to obtain the block copolymer polyol-MDI type low free prepolymer; the amount of the nano metal oxide is (0.1-1) wt.% of the total amount of the prepolymer components; The block copolymer polyol is one or more of Capa 7201A, Capa 8015D, Capa 8025D, Capa 8025E or Capa7203; The nano metal oxide is one of nano zinc oxide, nano aluminum oxide or nano magnesium oxide.
2. The polyurethane forklift wheel material with strong environmental adaptability according to claim 1, characterized in that: The small molecule polyol is one of 1,4-butanediol, trimethylolpropane, triethanolamine or ethylene glycol.
3. The polyurethane forklift wheel material with strong environmental adaptability according to claim 1, characterized in that: The bifunctional secondary amine p-phenylenediamine curing agent is one or more of absintheine, N,N-diisopropyl p-phenylenediamine, N,N'-di-sec-butyl p-phenylenediamine, 4,4-methylenebis(N-methylaniline) or 4,4'-bis-sec-butylaminodiphenylmethane.
4. The polyurethane forklift wheel material with strong environmental adaptability according to claim 1, characterized in that: The catalyst is one of DXD-06C, DXD-07C or CH-05.
5. The polyurethane forklift wheel material with strong environmental adaptability according to claim 1, characterized in that: The particle size of the nano metal oxide is 20-50nm.
6. The polyurethane forklift wheel material with strong environmental adaptability according to claim 1, characterized in that: The MDI type isocyanate is one or more of carbodiimide modified diphenylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, MDI-100 or MDI-50.
7. The polyurethane forklift wheel material with strong environmental adaptability according to claim 1, characterized in that: The polyurethane forklift wheel material with strong environmental adaptability has a room temperature hardness of ≥94A / 48D, a room temperature rebound rate of ≥50%, a low temperature rebound rate of ≥40%, and a right-angle tear strength of >120kN / m.
8. A method for preparing a polyurethane forklift wheel material with strong environmental adaptability according to any one of claims 1 to 7, characterized in that: Here are the steps: (1) Putting a small molecule polyol and a block copolymer polyol into a reaction kettle, vacuum dehydrating to a water content of ≤0.05wt.%, cooling to below 60°C, adding a difunctional secondary amine p-phenylenediamine type curing agent and a catalyst, and mixing evenly to obtain a curing agent component; (2) Add block copolymer polyol and MDI isocyanate in a mass ratio of (37.5-50.75): (49.25-62.5) into a reactor respectively, keep the reaction at 75-85°C for 2.5-3h, then add nano metal oxide and continue stirring, and vacuum degassing to obtain block copolymer polyol-MDI low free prepolymer; its -NCO content is (13-19) wt.%; (3) The curing agent component and the prepolymer component are kept warm at 60-65°C and 75-80°C respectively. When in use, the curing agent component and the prepolymer component are evenly mixed in a mass ratio of (39.5-44.4):100, poured into a mold at 101-110°C, and post-vulcanized at a temperature of 100-105°C for 16-20h after the mold is opened to obtain a polyurethane forklift wheel material with strong environmental adaptability.