A kind of biodegradable functional plastic particles and preparation method thereof

By using composite flame retardant plastic masterbatches and related additives, and by the composite of polylactic acid polyethylene glycol amino, graphene with grafted aminosilane coupling agent and modified DOPO, the biodegradation of plastic particles in the prior art is solved. The poor performance and lack of antibacterial flame retardant properties have achieved high thermal stability and good flame retardant properties.

CN118440478BActive Publication Date: 2024-11-29SHANDONG BLUE OCEAN CRYSTAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410680637.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-29
Publication Date
2024-11-29
Estimated Expiration
2044-05-29

AI Technical Summary

Technical Problem

In the prior art, plastic particles have poor biodegradability, lack of antibacterial and flame retardant effects, and when various functional components in plastic particles are combined, their integrity and stability are poor.

Method used

Graphene using composite flame retardant plastic masterbatch as the matrix, adding polyvinyl chloride, heat stabilizer, plasticizer, antioxidant and light stabilizer, and passing polylactic acid polyethylene glycol amino group and grafted aminosilane coupling agent Combination with modified DOPO, a crosslinked structure is formed to improve thermal stability and flame retardant properties.

Benefits of technology

The high thermal stability, good tensile strength and significant antibacterial flame retardant properties of biodegradable functional plastic particles are achieved, and the integrity and stability of plastic particles are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004865495040000041
    Figure BDA0004865495040000041
  • Figure BDA0004865495040000042
    Figure BDA0004865495040000042
  • Figure BDA0004865495040000051
    Figure BDA0004865495040000051
Patent Text Reader

Abstract

The invention discloses a biodegradable functional plastic particle and a preparation method thereof, belonging to the technical field of polymer materials, and used to solve the technical problems of poor biodegradability, poor antibacterial property and flame retardancy of plastic particles in the prior art; the invention comprises a composite flame retardant plastic masterbatch, polyvinyl chloride, a heat stabilizer, a plasticizer, an antioxidant and a light stabilizer; the composite flame retardant plastic masterbatch is prepared from polylactic acid polyethylene glycol amino, graphene grafted with an aminosilane coupling agent and modified DOPO; the modified DOPO is obtained by modifying citral; the modified DOPO is introduced to improve the flame retardancy of the plastic particles; the graphene grafted with an aminosilane coupling agent is introduced to improve the flame retardancy of the plastic particles; the components of the composite flame retardant plastic masterbatch are mixed and reacted to generate a cross-linked structure, thereby improving the thermal stability of the prepared plastic particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a biodegradable functional plastic particle and a preparation method thereof. Background Art

[0002] Plastics, rubber and synthetic fibers are collectively referred to as the three major synthetic materials, among which plastics have the widest application range. However, traditional plastics represented by PE and PP have relatively stable molecular structures and poor degradation capabilities in natural conditions such as soil or ocean. Harmful substances produced by discarded plastics enter the food chain through the ecosystem, endangering the health of animals and plants. White pollution has become a major challenge facing the development of polymer materials. Biodegradable plastics can not only overcome the dependence of plastic products on traditional petroleum-based non-degradable materials, but also will not pollute the environment. They are the most effective solution to the problem of white pollution.

[0003] Plastics represented by PVC have poor flame retardant properties and will produce a large amount of toxic and harmful smoke during combustion. Therefore, flame retardant plastics need to be further developed to meet the safety and health needs of plastic applications. In addition, pathogenic infectious diseases and food safety issues caused by the contamination and growth of pathogenic microorganisms are also one of the public hazards that threaten human health. In order to avoid the occurrence of foodborne infectious diseases and extend the shelf life, plastics containing antibacterial substances are an important research direction in the future.

[0004] Patent application CN115109276A discloses a production process of environmentally friendly degradable plastic particles, which comprises mixing and extruding modified polystyrene, nanocellulose, paraffin wax, and flame retardant, cooling and granulating to obtain environmentally friendly degradable plastic particles, reacting chloroacetyl chloride with polystyrene with alkyl halides, and then reacting with ethylenediamine to obtain aminopolystyrene, and then subjecting the aminopolystyrene to a series of modification treatments, and reacting with polylactic acid polyethylene glycol amino groups and sorbitol in sequence to obtain plastic particles with good biodegradability;

[0005] However, the above-mentioned environmentally friendly and degradable plastic particles use inorganic flame retardants such as aluminum hydroxide, magnesium hydroxide, and ammonium polyphosphate. The inorganic flame retardants have poor compatibility with various organic components, which reduces the thermal stability of the prepared environmentally friendly and degradable plastic particles.

[0006] Patent application CN109337315A discloses a green biodegradable plastic masterbatch and its processing technology, which uses polylactic acid as the plastic masterbatch base, supplemented with modified phenolic resin, polyester elastomer, bamboo charcoal particles, polyethylene glycol and chitosan. The prepared plastic masterbatch has the advantages of green biodegradability and good mechanical properties.

[0007] However, the above-mentioned prior art only improves the biodegradability of the prepared plastic particles, but fails to prepare functional plastics with antibacterial and flame retardant properties.

[0008] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0009] The purpose of the present invention is to provide a biodegradable functional plastic particle and a preparation method thereof, which is used to solve the problems in the prior art of poor biodegradability of plastic particles, lack of antibacterial and flame retardant effects, and poor integrity and stability of the plastic particles when the functional components in the plastic particles are compounded.

[0010] The purpose of the present invention can be achieved through the following technical scheme: a biodegradable functional plastic particle, which comprises, by weight, 70-80 parts of a composite flame retardant plastic masterbatch, 10-20 parts of polyvinyl chloride, 0.5-1 parts of a heat stabilizer, 5-10 parts of a plasticizer, 0.5-1 parts of an antioxidant and 1-3 parts of a light stabilizer.

[0011] The present invention uses composite flame retardant plastic masterbatch as base particle and polyvinyl chloride material as auxiliary particle. Due to the existence of allyl structure on the polyvinyl chloride macromolecular chain, heat stabilizer and light stabilizer need to be added. Antioxidant and plasticizer are two other important auxiliary agents added when preparing plastic.

[0012] Furthermore, the composite flame retardant plastic masterbatch is prepared by the following steps:

[0013] The polylactic acid polyethylene glycol amino is vacuum dried, the graphene grafted with an amino silane coupling agent is dried, and then the polylactic acid polyethylene glycol amino, the graphene grafted with an amino silane coupling agent and the modified DOPO are mixed, melt-blended and extruded into granules in a twin-screw extruder to obtain a composite flame-retardant plastic masterbatch.

[0014] Graphene grafted with aminosilane coupling agent and modified DOPO can react with the carboxyl group in the amino group of polylactic acid polyethylene glycol, so as to obtain a composite flame retardant plastic masterbatch of the three in a melt blending process.

[0015] Furthermore, in terms of weight, the usage ratio of polylactic acid polyethylene glycol amino, graphene grafted with amino silane coupling agent and modified DOPO is 70-80:10-20:10-20; the vacuum drying temperature of polylactic acid polyethylene glycol amino is 70-75°C, and the vacuum drying time is 10-12h; the drying temperature of graphene grafted with amino silane coupling agent is 60°C, and it is dried to constant weight; the melt blending temperature is 180-220°C, and the melt blending time is 10-15min.

[0016] Further, the graphene grafted with an aminosilane coupling agent is prepared by the following steps:

[0017] S1, graphene oxide powder and SOCl2 are mixed and stirred evenly, then heated to 50-60°C, mixed and reacted for 30-60 minutes to obtain a mixed solid-liquid; then filtered, washed with deionized water, and vacuum dried to constant weight to obtain acylated graphene;

[0018] S2. Using ethanol as solvent, a 3-10% wt aminosilane coupling agent solution is prepared; acylated graphene is immersed in the 3-10% wt aminosilane coupling agent solution, reacted at a constant temperature of 60° C. for 60-100 min, and then filtered to obtain a solid; the solid is repeatedly washed and dried with anhydrous ethanol to obtain graphene grafted with an aminosilane coupling agent.

[0019] Graphene oxide is a thin layer supported by a carbon skeleton, the basal surface of which is modified by hydroxyl and epoxy groups, and the edges are randomly occupied by carboxyl and carbonyl groups, forming a mixed SP 2 -SP 3 Carbon system, graphene oxide and SOCl2 undergo acyl halide reaction, and the carboxyl group is halogenated into acyl halide.

[0020] The reaction principle of graphene oxide powder and SOCl2 is as follows:

[0021]

[0022] The acyl halide functional group of the graphene and the amino group of the aminosilane coupling agent undergo an amidation reaction to prepare graphene grafted with the aminosilane coupling agent.

[0023] Taking 3-aminopropyltriethoxysilane as an example, the reaction principle of acylated graphene and 3-aminopropyltriethoxysilane is as follows:

[0024]

[0025] Further, in step S1, the ratio of graphene oxide powder to SOCl2 is 5-10 g:10-15 mL; in step S2, the ratio of acylated graphene powder to aminosilane coupling agent is 15-20 g:100 mL;

[0026] Furthermore, in step S2, the aminosilane coupling agent is any one of 3-aminopropyltriethoxysilane, di(3-trimethoxysilylpropyl)amine, diethylenetriaminopropyltrimethoxysilane, 1H,1H,1H,1H-perfluorodecyltrimethoxysilane, and n-octyltriethoxysilane, and a combination thereof.

[0027] Furthermore, the preparation method of the modified DOPO comprises the following steps:

[0028] Citral and ethanol are mixed and dissolved, and DOPO is added and ultrasonically dispersed to obtain a mixed system; the mixed system is reacted at 50-60°C and condensed under reflux for 4-5 hours, and after the reaction is completed, it is cooled to room temperature to obtain a mixed solid-liquid; the mixed solid-liquid is filtered to obtain a solid; the solid is vacuum dried, and then ground and sieved to obtain a modified DOPO.

[0029] The phosphate group of DOPO acts as a nucleophile and undergoes an addition reaction with the aldehyde group to prepare modified DOPO.

[0030] The reaction mechanism of DOPO and aldehyde groups is as follows:

[0031]

[0032] Furthermore, the dosage ratio of citral, ethanol and DOPO is 15-30mL:50mL:20g; the solid vacuum drying temperature is 70-75°C, and the vacuum drying is performed to constant weight; and the mesh size of the ground sieve is 300 mesh.

[0033] As another aspect of the present invention, the present invention also provides a method for preparing biodegradable functional plastic particles, comprising the following steps:

[0034] A1, composite flame retardant plastic masterbatch, polyvinyl chloride, heat stabilizer, plasticizer, antioxidant and light stabilizer are added into a high-speed mixer and mixed at high speed for 5 minutes at room temperature to obtain raw materials;

[0035] A2. Add the raw materials to a torque rheometer for melt blending to obtain a blend; crush the blend using a plastic crusher to obtain particles with a particle size of 1-2 mm; add the particles to an injection molding machine for injection molding to obtain a biodegradable functional plastic particle.

[0036] The composite flame retardant plastic masterbatch, polyvinyl chloride and related additives are pre-mixed to obtain raw materials for preparing plastic particles. The raw materials are then melt-blended, crushed and injection-molded through a series of process equipment and process operations to obtain biodegradable functional plastic particles.

[0037] Furthermore, in step A2, the speed of the torque rheometer is set to 40-50 rpm, the temperature of melt blending is 170-180°C, and the time of melt blending is 6-10 min; the pressure of injection molding is 10-15 MPa, the temperature of zone 1 of the injection molding machine is 130°C, and the temperature of zone 2 is set to 140-150°C.

[0038] The composite flame retardant plastic is passed through an internal mixer, a torque rheometer and other processing equipment, and the composite flame retardant plastic and various processing aids are mixed by utilizing high-speed stirring and high-temperature characteristics, thereby forming plastic particles with excellent biodegradable performance.

[0039] The present invention has the following beneficial effects:

[0040] 1. The present invention uses composite flame-retardant plastic masterbatch as the matrix of biodegradable functional plastic particles prepared, and a certain amount of polyvinyl chloride is added to obtain plastic materials. Due to the doping of polyvinyl chloride, irregularly distributed thermal decomposition initiation sources-allyl chloride structures exist on the polyvinyl chloride macromolecular chains, so heat stabilizers and light stabilizers are added. Plasticizers and antioxidants are two other important auxiliary agents for preparing plastic particles. Polylactic acid polyethylene glycol amino, graphene grafted with aminosilane coupling agent and modified DOPO are composited to obtain composite flame-retardant plastic masterbatch. Graphene is used as a flame-retardant material, and aminosilane coupling agent is introduced to improve the dispersibility of graphene on the matrix. DOPO itself is flame-retardant, and citral is introduced to improve antibacterial properties. Polylactic acid polyethylene glycol amino, graphene grafted with aminosilane coupling agent and modified DOPO react to produce a cross-linked structure, thereby improving the thermal stability of the prepared plastic particles.

[0041] 2. Graphene itself has good thermal properties and plays a role of barrier protection when the polymer is thermally decomposed. The special structure of graphene itself can be compounded with polylactic acid polyethylene glycol amino. After the acylated graphene powder is grafted with aminosilane coupling agent, the introduction of silicon element further increases the flame retardant properties of the graphene powder. In addition, the dispersibility of graphene itself in polylactic acid polyethylene glycol amino is poor. The present invention combines aminosilane coupling agent and graphene, which helps to evenly disperse graphene in polylactic acid polyethylene glycol amino.

[0042] Citral itself has significant antifungal and bactericidal effects, but citral has poor stability and is prone to chemical degradation under low pH and oxidative conditions. The present invention uses DOPO to modify citral to obtain modified DOPO, which helps to improve the stability of citral itself. On the one hand, DOPO, as a high-efficiency flame retardant, improves the flame retardant efficiency of preparing composite flame-retardant plastic masterbatch. On the other hand, the hydroxyl and double bond functional groups in the modified DOPO can generate charge attraction with the chlorine atoms in polyvinyl chloride, thereby improving the integrity and stability of the prepared composite flame-retardant plastic masterbatch and polyvinyl chloride auxiliary materials.

[0043] 3. The present invention also selects polylactic acid polyethylene glycol amino as the base particle of biodegradable functional plastic particles, thereby improving the degradation performance of the prepared biodegradable functional plastic particles. The biodegradable functional plastic particles prepared in Example 3 were buried in the soil for 21 days, and the degradation rate reached 13.4%. Polylactic acid polyethylene glycol amino was selected to replace single polylactic acid, and the amino functional group of polylactic acid polyethylene glycol amino was mixed with graphene grafted with aminosilane coupling agent and modified DOPO to produce a cross-linked structure, thereby improving the thermal stability of the prepared biodegradable functional plastic particles. DETAILED DESCRIPTION

[0044] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0045] Example 1

[0046] This embodiment provides a method for preparing biodegradable functional plastic particles, comprising the following steps:

[0047] Step 1: Preparation of acylated graphene

[0048] 5 g of graphene oxide powder and 10 mL of SOCl2 were added to a 50 mL three-necked round-bottom flask, mixed and stirred evenly, then transferred to a water bath, heated to 50 ° C, and stirred at 100 r / min for 30 min to obtain a mixed solid-liquid; then filtered, washed three times with deionized water, and vacuum dried to constant weight to obtain acylated graphene.

[0049] Step 2: Preparation of graphene grafted with aminosilane coupling agent

[0050] Using ethanol as solvent, a 3%wt aminosilane coupling agent solution is prepared; 15g of acylated graphene is immersed in 100mL of the 3%wt aminosilane coupling agent solution, heated at a constant temperature of 60°C for 60min, and then filtered to obtain a solid; the solid is repeatedly washed with anhydrous ethanol and dried to obtain graphene grafted with an aminosilane coupling agent.

[0051] Step 3: Preparation of modified DOPO

[0052] 15 mL of citral and 50 mL of ethanol were added to a 250 mL three-necked flask and dissolved in each other. Then 20 g of DOPO was added to the three-necked flask and ultrasonically dispersed for 10 min to obtain a mixed system. The three-necked flask was placed on a water bath with the water bath temperature set to 50 ° C. Under condensation reflux conditions, magnetic stirring was carried out at 100 r / min for 4 h. After the reaction was completed, it was naturally cooled to room temperature to obtain a mixed solid-liquid mixture; the mixed solid-liquid mixture was filtered to obtain a solid. The solid was vacuum dried at 50 ° C to constant weight, and then ground through a 300 mesh sieve to obtain a modified DOPO.

[0053] Step 4: Preparation of composite flame retardant plastic masterbatch

[0054] The polylactic acid polyethylene glycol amino was placed in an oven at 70°C for vacuum drying for 10 hours, and the graphene grafted with aminosilane coupling agent was dried in an oven at 80°C for 4 hours. The modified DOPO, graphene grafted with aminosilane coupling agent and polylactic acid polyethylene glycol amino were then blended, wherein the modified DOPO was 70 parts, the graphene grafted with aminosilane coupling agent was 10 parts, and the polylactic acid polyethylene glycol amino was 10 parts; then the mixture was melt-blended and extruded into granules in a twin-screw extruder to obtain a composite flame-retardant plastic masterbatch; wherein the temperature of the melt blending was 180°C and the time of the melt blending was 10 minutes.

[0055] Step 5: Preparation of biodegradable functional plastic particles

[0056] 50 parts of composite flame retardant plastic masterbatch, 0.5 parts of heat stabilizer, 1 part of plasticizer, 0.1 parts of antioxidant and 0.1 parts of light stabilizer were added to a high-speed mixer and mixed evenly at room temperature for 5 minutes to obtain raw materials. 50g of raw materials were weighed and added to a torque rheometer for melt blending to obtain a blend; wherein the melting temperature was 170°C, the speed of the torque rheometer was set to 40rpm, and the melting time was 6 minutes. The blend was crushed by a plastic crusher to obtain particles with a particle size of 1mm; the particles were added to an injection molding machine for injection molding to obtain a biodegradable functional plastic particle; wherein the injection pressure was set to 10MPa, the temperature of the first zone was 130°C, and the temperature of the second zone was set to 140°C.

[0057] Example 2

[0058] This embodiment provides a method for preparing biodegradable functional plastic particles, comprising the following steps:

[0059] Step 1: Preparation of acylated graphene

[0060] 8 g of graphene oxide powder and 12 mL of SOCl2 were added to a 50 mL three-necked round-bottom flask, mixed and stirred evenly, then transferred to a water bath, heated to 55 ° C, and stirred at 100 r / min for 50 min to obtain a mixed solid-liquid; then filtered, washed three times with deionized water, and vacuum dried to constant weight to obtain acylated graphene.

[0061] Step 2: Preparation of graphene grafted with aminosilane coupling agent

[0062] Using ethanol as solvent, a 3%wt aminosilane coupling agent solution is prepared; 16g of acylated graphene is immersed in 100mL of a 5%wt aminosilane coupling agent solution, heated at a constant temperature of 60°C for 80min, and then filtered to obtain a solid; the solid is repeatedly washed with anhydrous ethanol and dried to obtain graphene grafted with an aminosilane coupling agent.

[0063] Step 3: Preparation of modified DOPO

[0064] 25 mL of citral and 50 mL of ethanol were added to a 250 mL three-necked flask and dissolved in each other. Then 20 g of DOPO was added to the three-necked flask and ultrasonically dispersed for 10 min to obtain a mixed system. The three-necked flask was placed on a water bath with the water bath temperature set to 56 ° C. Under the condition of condensation reflux, magnetic stirring was carried out at 100 r / min for 4.5 h. After the reaction was completed, it was naturally cooled to room temperature to obtain a mixed solid-liquid mixture; the mixed solid-liquid mixture was filtered to obtain a solid. The solid was vacuum dried at 54 ° C to constant weight, and then ground through a 300 mesh sieve to obtain a modified DOPO.

[0065] Step 4: Preparation of composite flame retardant plastic masterbatch

[0066] The polylactic acid polyethylene glycol amino was placed in an oven at 73°C for vacuum drying for 11 hours, the graphene grafted with an aminosilane coupling agent was dried to constant weight, and the polylactic acid polyethylene glycol amino was dried in an oven at 90°C for 4.4 hours. The modified DOPO, the graphene grafted with an aminosilane coupling agent and the polylactic acid polyethylene glycol amino were then blended, wherein the modified DOPO was 70 parts, the graphene grafted with an aminosilane coupling agent was 10 parts, and the polylactic acid polyethylene glycol amino was 10 parts. The mixture was then melt-blended and extruded into granules in a twin-screw extruder to obtain a composite flame-retardant plastic masterbatch; wherein the temperature of the melt blending was 200°C and the time of the melt blending was 12 minutes.

[0067] Step 5: Preparation of biodegradable functional plastic particles

[0068] 57 parts of composite flame retardant plastic masterbatch, 0.8 parts of heat stabilizer, 1 part of plasticizer, 0.4 parts of antioxidant and 0.3 parts of light stabilizer were added to a high-speed mixer and mixed evenly at room temperature for 6 minutes to obtain raw materials. 50g of raw materials were weighed and added to a torque rheometer for melt blending to obtain a blend; wherein the melting temperature was 176°C, the speed of the torque rheometer was set to 44rpm, and the melting time was 8min. The blend was crushed by a plastic crusher to obtain particles with a particle size of 1.5mm; the particles were added to an injection molding machine for injection molding to obtain a biodegradable functional plastic particle; wherein the injection pressure was set to 12MPa, the temperature of the first zone was 130°C, and the temperature of the second zone was set to 147°C.

[0069] Example 3

[0070] This embodiment provides a method for preparing biodegradable functional plastic particles, comprising the following steps:

[0071] Step 1: Preparation of acylated graphene

[0072] 10 g of graphene oxide powder and 15 mL of SOCl2 were added to a 50 mL three-necked round-bottom flask, mixed and stirred evenly, then transferred to a water bath, heated to 60 ° C, and stirred at 100 r / min for 60 min to obtain a mixed solid-liquid; then filtered, washed three times with deionized water, and vacuum dried to constant weight to obtain acylated graphene.

[0073] Step 2: Preparation of graphene grafted with aminosilane coupling agent

[0074] Using ethanol as solvent, a 10%wt aminosilane coupling agent solution is prepared; 20g of acylated graphene powder is immersed in 100mL of the 10%wt aminosilane coupling agent solution, heated at a constant temperature of 60°C for 100min, and then filtered to obtain a solid; the solid is repeatedly washed with anhydrous ethanol and dried to obtain graphene grafted with the aminosilane coupling agent.

[0075] Step 3: Preparation of modified DOPO

[0076] 30 mL of citral and 50 mL of ethanol were added to a 250 mL three-necked flask and dissolved in each other. Then 20 g of DOPO was added to the three-necked flask and ultrasonically dispersed for 10 min to obtain a mixed system. The three-necked flask was placed on a water bath, the water bath temperature was set to 60 ° C, and magnetic stirring was performed at 100 r / min for 5 h under condensation reflux conditions. After the reaction was completed, it was naturally cooled to room temperature to obtain a mixed solid-liquid; the mixed solid-liquid was filtered to obtain a solid. The solid was vacuum dried at 60 ° C for 24 h, and then ground through a 300 mesh sieve to obtain a modified DOPO.

[0077] Step 4: Preparation of composite flame retardant plastic masterbatch

[0078] The polylactic acid polyethylene glycol amino was placed in an oven at 75°C for vacuum drying for 12 hours, the graphene grafted with an aminosilane coupling agent was dried to constant weight, and the polylactic acid polyethylene glycol amino was dried in an oven at 100°C for 5 hours, and then 20 parts of modified DOPO, 20 parts of graphene grafted with an aminosilane coupling agent and 80 parts of polylactic acid polyethylene glycol amino were blended, wherein the modified DOPO was 70 parts, the graphene grafted with an aminosilane coupling agent was 10 parts, and the polylactic acid polyethylene glycol amino was 10 parts, and then melt-blended and extruded into granules in a twin-screw extruder to obtain a composite flame-retardant plastic masterbatch; wherein the temperature of the melt blending was 220°C and the time of the melt blending was 15 minutes.

[0079] Step 5: Preparation of biodegradable functional plastic particles

[0080] 60 parts of composite flame retardant plastic masterbatch, 1 part of heat stabilizer, 2 parts of plasticizer, 0.5 parts of antioxidant and 0.5 parts of light stabilizer were added to a high-speed mixer and mixed evenly at room temperature for 10 minutes to obtain raw materials. 50g of raw materials were weighed and added to a torque rheometer for melt blending to obtain a blend; wherein the melting temperature was 180°C, the speed of the torque rheometer was set to 50rpm, and the melting time was 10min. The blend was crushed by a plastic crusher to obtain particles with a particle size of 2mm; the particles were added to an injection molding machine for injection molding to obtain a biodegradable functional plastic particle; wherein the injection pressure was set to 15MPa, the temperature of the first zone was 130°C, and the temperature of the second zone was set to 150°C.

[0081] Comparative Example 1

[0082] Compared with Example 3, this comparative example eliminates step 2, and uses acylated graphene instead of graphene grafted with an aminosilane coupling agent.

[0083] Comparative Example 2

[0084] Compared with Example 3, this comparative example eliminates step 3, and DOPO is not modified with citral.

[0085] Comparative Example 3

[0086] Compared with Example 3, in step 4, the polylactic acid polyethylene glycol amino group is replaced with polylactic acid of equal mass.

[0087] Comparative Example 4

[0088] Compared with Example 3, in step 4, the polylactic acid polyethylene glycol amino group is replaced by polyethylene of the same mass.

[0089] Performance Testing:

[0090] 1. According to GB / T14402-2007, 10 mg of the biodegradable functional plastic particles prepared in Examples 1-3 and Comparative Examples 1-3 were placed in a small alumina crucible. Under the protection of a nitrogen atmosphere, the temperature was raised from room temperature to 400°C at a heating rate of 20°C / min. The mass preservation rate of the biodegradable functional plastic particles prepared in Examples 1-3 and Comparative Examples 1-3 was calculated.

[0091] 2. According to GB / T1040.1-2018 "Determination of tensile properties of plastics", the WDW universal tensile testing machine was used to test the tensile properties and obtain the tensile strength; the tensile rate was 5 mm / min, and each group of samples was tested 5 times to obtain the average value.

[0092] 3. Staphylococcus aureus was selected as the test bacteria, and the antibacterial effect of the biodegradable functional plastic particles prepared in Examples 1-3 and Comparative Examples 1-3 was quantitatively evaluated by plate counting method.

[0093] 4. Select 6 small flower pots of the same size and fill them with soil. Weigh 10 g of the biodegradable functional plastic particles prepared in Examples 1-3 and Comparative Examples 1-3 and bury them in the soil at a depth of 10 cm. Take out the biodegradable functional plastic particles after 21 days, wash them with deionized water, put them in a vacuum oven at 40°C and dry them overnight to constant weight, weigh them, and calculate the degradation rate.

[0094] Degradation rate ω=(M0-M n ) / t×100%

[0095] Where: t is the degradation time of biodegradable functional plastic particles in soil; M n is the mass of the degraded biodegradable functional plastic particles after drying; M0 is the initial mass of the biodegradable functional plastic particles.

[0096] The specific test results are shown in the table below:

[0097] Table 1

[0098]

[0099] Data Analysis:

[0100] Comparative analysis of the data in the above table shows that the biodegradable functional plastic particles prepared in Examples 1-3 of the present invention all have excellent thermal stability and tensile strength, as shown by the high mass preservation rate and tensile strength values ​​of the biodegradable functional plastic particles prepared in Examples 1-3;

[0101] In Comparative Example 1, acylated graphene was used to replace the graphene grafted with an aminosilane coupling agent, and in Comparative Example 3, the polylactic acid polyethylene glycol amino group was replaced with polylactic acid of equal mass, which was not conducive to the organic connection between the components, thereby reducing the stability and tensile strength of the prepared biodegradable functional plastic particles;

[0102] In Comparative Example 2, DOPO was not modified with citral, and the antibacterial activity of the obtained biodegradable functional plastic particles against Staphylococcus aureus was reduced. In Comparative Example 4, polyethylene of equal quality and difficult to degrade was used to replace polylactic acid polyethylene glycol amino, and the degradation rate of the prepared biodegradable functional plastic particles was reduced, and the degradation rate after 21 days was only 8.5%.

[0103] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0104] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0105] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A biodegradable functional plastic particle, characterized in that: According to weight parts, it includes 70-80 parts of composite flame retardant plastic masterbatch, 10-20 parts of polyvinyl chloride, 0.5-1 parts of heat stabilizer, 5-10 parts of plasticizer, 0.5-1 parts of antioxidant and 1-3 parts of light stabilizer; The composite flame retardant plastic masterbatch is prepared by the following steps: The polylactic acid polyethylene glycol amino group is vacuum dried, and the graphene grafted with an amino silane coupling agent is dried; then the polylactic acid polyethylene glycol amino group, the graphene grafted with an amino silane coupling agent and the modified DOPO are mixed, melt-blended and extruded into granules in a twin-screw extruder to obtain a composite flame-retardant plastic masterbatch; The preparation method of the modified DOPO comprises the following steps: Citral and ethanol are mixed and dissolved in each other, and DOPO is then added and ultrasonically dispersed to obtain a mixed system; the mixed system is condensed and refluxed at 50-60°C for 4-5 hours, and after the reaction is completed, it is cooled to room temperature to obtain a mixed solid-liquid; the mixed solid-liquid is filtered to obtain a solid; the solid is vacuum dried, and then ground and sieved to obtain a modified DOPO.

2. The biodegradable functional plastic particles according to claim 1, characterized in that: According to weight proportion, the usage ratio of polylactic acid polyethylene glycol amino, graphene grafted with amino silane coupling agent and modified DOPO is 70-80:10-20:10-20; the vacuum drying temperature of polylactic acid polyethylene glycol amino is 70-75°C, and the vacuum drying time is 10-12h; the drying temperature of graphene grafted with amino silane coupling agent is 60°C, and dried to constant weight; the temperature of melt blending is 180-220°C, and the melt blending time is 10-15min.

3. The biodegradable functional plastic particles according to claim 1, characterized in that: Graphene grafted with an aminosilane coupling agent is prepared by the following steps: S1, graphene oxide powder and SOCl2 are mixed and stirred evenly, then heated to 50-60°C, mixed and reacted for 30-60 minutes to obtain a mixed solid-liquid; then filtered, washed with deionized water, and vacuum dried to constant weight to obtain acylated graphene; S2. Using ethanol as solvent, prepare a 3-10%wt aminosilane coupling agent solution; immerse the acylated graphene in the 3-10%wt aminosilane coupling agent solution, react at a constant temperature of 60°C for 60-100min, and then filter to obtain a solid; the solid is repeatedly washed and dried with anhydrous ethanol to obtain graphene grafted with an aminosilane coupling agent.

4. The biodegradable functional plastic particles according to claim 3, characterized in that: In step S1, the amount ratio of graphene oxide powder and SOCl2 is 5-10g:10-15mL; in step S2, the amount ratio of acylated graphene powder and aminosilane coupling agent is 15-20g:100mL.

5. The biodegradable functional plastic particles according to claim 3, characterized in that: In step S2, the aminosilane coupling agent is any one of 3-aminopropyltriethoxysilane, di(3-trimethoxysilylpropyl)amine, and diethylenetriaminepropyltrimethoxysilane, and a combination thereof.

6. The biodegradable functional plastic particles according to claim 1, characterized in that: The dosage ratio of citral, ethanol and DOPO is 15-30mL:50mL:20g; the solid vacuum drying temperature is 70-75°C and vacuum drying is performed to constant weight; the mesh size of the ground and sieved is 300 meshes.

7. A method for preparing a biodegradable functional plastic particle according to any one of claims 1 to 6, characterized in that: The following steps are involved: A1, composite flame retardant plastic masterbatch, heat stabilizer, plasticizer, antioxidant and light stabilizer are added into a high-speed mixer and mixed evenly to obtain raw materials; A2. Add the raw materials to a torque rheometer for melt blending to obtain a blend; crush the blend using a plastic crusher to obtain particles with a particle size of 1-2 mm; add the particles to an injection molding machine for injection molding to obtain a biodegradable functional plastic particle.

8. The method for preparing biodegradable functional plastic particles according to claim 7, characterized in that: In step A1, the heat stabilizer is any one of tribasic lead sulfate, dibasic lead sulfate, dibasic lead maleate, and basic lead carbonate, and their combinations; the plasticizer is any one of dibutyl phthalate, dibutyl phthalate, dioctyl adipate, epoxy soybean oil, and tricresyl phosphate, and their combinations; the antioxidant is any one of antioxidant 264, antioxidant 1076, antioxidant 425, and antioxidant 330, and their combinations; the light stabilizer is any one of UV-9, UV-531, UV-327, and UV-1084, and their combinations; In step A2, the speed of the torque rheometer is set to 40-50 rpm, the temperature of melt blending is 170-180°C, and the time of melt blending is 6-10 min; the pressure of injection molding is 10-15 MPa, the temperature of zone 1 of the injection molding machine is 130°C, and the temperature of zone 2 is set to 140-150°C.

Citation Information

Patent Citations

  • Green biodegradable plastic master batch and processing process thereof

    CN109337315A

  • Production process of environment-friendly degradable plastic particles

    CN115109276A

  • Degradable environment-friendly plastic

    CN104650506A

  • Biobased modifiers for polyvinylchloride blends

    US20140051787A1