Sodium ion battery positive electrode material and preparation method and application thereof

By optimizing the proportion and structure of the sodium-ion battery cathode material, the high voltage drop and safety issues of traditional sodium-ion batteries under high-rate conditions are solved, high-rate performance and cycle stability are achieved, and the application of sodium-ion batteries is improved. Advantages.

CN118448628BActive Publication Date: 2024-10-29NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410854158.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Traditional sodium-ion batteries have a high voltage drop under the condition of 5C charge and discharge rate, which leads to performance degradation, safety issues, and low rate, which limits its application in the field of start-stop power supply.

Method used

Develop a sodium-ion battery cathode material with the general chemical formula NaaLigNibFecMndAeCofO2. It is sintered through specific ratios and element combinations, including low-melting point sodium sources, lithium sources and compounds containing A elements, to form a layered structure, and is combined with cobalt sources. Secondary sintering optimizes the sodium ratio and Na-O layer spacing to improve rate and cycle stability.

Benefits of technology

The voltage drop of the sodium-ion battery under 5C charging and discharging conditions is achieved to be as low as 6.5%, which improves the rate and cycle stability, extends the battery life, reduces the resistance, and enhances safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118448628B_ABST
    Figure CN118448628B_ABST
Patent Text Reader

Abstract

The present invention relates to a sodium ion battery positive electrode material and a preparation method and application thereof. The chemical general formula of the sodium ion battery positive electrode material is Na a Li g Ni b Fe c Mn d A e Co f O2, wherein 1.05≤a≤1.15, 0.2≤b≤0.4, 0.2≤c≤0.4, 0.2≤d≤0.4, 0.0001≤e≤0.005, 0.0002≤f≤0.004, 0.02≤g≤0.2, and a / (b+c+d) is 1.05-1.15, A is an element with an ion radius greater than or equal to 0.080nm, and the Na-O interlayer spacing is 3.00Å-3.16Å. The sodium ion battery positive electrode material of the present invention has excellent high rate performance and cycle stability, and improves the application advantages of sodium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery positive electrode material and a preparation method and application thereof. Background Art

[0002] Sodium-ion batteries have excellent low-temperature performance and cycle performance, and have great application potential in the field of start-stop power supplies. However, under the condition of 5C charge and discharge rate, the voltage drop of traditional sodium-ion batteries is as high as more than 15%, which not only makes the battery performance prone to degradation and leads to a short battery life, but also causes battery overheating, gasification, liquefaction, and even fire and other safety issues. In order to improve the application advantages of sodium-ion batteries in the field of start-stop power supplies, it is urgent to develop a sodium-ion battery positive electrode material with high rate performance. Summary of the invention

[0003] Based on this, it is necessary to provide a sodium ion battery positive electrode material and a preparation method and application thereof to address the above problems; the sodium ion battery positive electrode material has excellent high rate performance and cycle stability, which improves the application advantages of sodium ion batteries.

[0004] A sodium ion battery positive electrode material, the chemical formula of the sodium ion battery positive electrode material is Na a Li g Ni b Fe c Mn d A e Co f O2, wherein 1.05≤a≤1.15, 0.2≤b≤0.4, 0.2≤c≤0.4, 0.2≤d≤0.4, 0.0001≤e≤0.005, 0.0002≤f≤0.004, 0.02≤g≤0.2, and a / (b+c+d) is 1.05-1.15, A is an element with an ionic radius greater than or equal to 0.080nm, and the Na-O interlayer spacing is 3.00Å-3.16Å.

[0005] In one embodiment, a / (b+c+d) is 1.06-1.14.

[0006] In one embodiment, the A element is selected from at least one of Sr, Y, K, Ca, Ce, and Rb.

[0007] In one embodiment, the sodium ion battery positive electrode material is a layered structure, and Co is distributed on the surface of the sodium ion battery positive electrode material.

[0008] A method for preparing the above-mentioned sodium ion battery positive electrode material comprises:

[0009] According to Naa Li g Ni b Fe c Mn d A e Co f O2, wherein 1.05≤a≤1.15, 0.2≤b≤0.4, 0.2≤c≤0.4, 0.2≤d≤0.4, 0.0001≤e≤0.005, 0.0002≤f≤0.004, 0.02≤g≤0.2, and a / (b+c+d) is a ratio of 1.05-1.15, a nickel iron manganese hydroxide precursor, a sodium source, a lithium source and a compound containing an element A are mixed and sintered once to obtain a pre-product, A is an element having an ion radius greater than 0.080 nm, and the sodium source includes a first sodium source having a melting point less than or equal to 350° C., and the molar fraction of the first sodium source in the sodium source is 1.5%-20%;

[0010] The pre-product is mixed with a cobalt source and subjected to secondary sintering to obtain the sodium ion battery positive electrode material.

[0011] In one embodiment, the first sodium source is selected from at least one of sodium oxalate, sodium acetate, sodium bicarbonate, and sodium nitrate.

[0012] In one embodiment, the sodium source further includes a second sodium source having a melting point greater than or equal to 800° C., and the second sodium source is selected from at least one of sodium carbonate, sodium oxide, sodium chloride, and sodium sulfate.

[0013] In one embodiment, the molar ratio of sodium ions in the second sodium source to sodium ions in the first sodium source is 5:1-50:1.

[0014] In one embodiment, the lithium source is selected from at least one of lithium carbonate, lithium hydroxide, and lithium oxalate;

[0015] And / or, element A is at least one selected from Sr, Y, K, Ca, Ce, and Rb.

[0016] In one embodiment, the primary sintering temperature is 880°C-980°C, and the time is 6h-14h;

[0017] And / or, the secondary sintering is carried out at a temperature of 700° C.-900° C. and for a time of 6 h-14 h.

[0018] A positive electrode sheet comprises the above-mentioned positive electrode material for a sodium ion battery.

[0019] A sodium ion battery comprises the positive electrode sheet as described above.

[0020] An electrical device comprises the sodium ion battery as described above.

[0021] The sodium ion battery positive electrode material of the present invention has a sodium ratio of 1.05-1.15 and a Na-O interlayer spacing of 3.00Å-3.16Å, and the grain boundary is enriched with A elements with an ion radius greater than or equal to 0.080nm. On the one hand, it overcomes the technical difficulties such as excessive alkali content caused by traditional high sodium content and thus low rate, so that the sodium ion battery positive electrode material has both high sodium ratio and low residual alkali content, thereby improving the rate and cycle stability of the sodium ion battery positive electrode material; on the other hand, the sodium ions in the sodium ion battery positive electrode material are easy to be deintercalated, which is beneficial to improve the capacity, and the synergistic effect between the elements in the sodium ion battery positive electrode material is not only beneficial to further improve the rate, but also improve the interface electronic conductivity, which is beneficial to reduce the resistance.

[0022] Therefore, the sodium ion battery positive electrode material of the present invention has excellent high-rate performance and cycle stability, and has high capacity and low resistance. When used in sodium ion batteries under the condition of a charge and discharge rate of 5C, the voltage drop is as low as within 6.5%, thereby improving the application advantages of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 The cross-sectional element distribution spectrum (EDS) test diagram and line data diagram of the sodium ion battery positive electrode material prepared in Example 1, wherein a is the cross-sectional image of the positive electrode material to be tested, and b is the corresponding spectrum Figure 1 To the mass fraction line data graph of cobalt element in spectrum 11;

[0025] Figure 2 This is a scanning electron microscope image of the sodium ion battery positive electrode material prepared in Example 1 under a magnification of 10K;

[0026] Figure 3 This is a scanning electron microscope image of the sodium ion battery positive electrode material prepared in Comparative Example 1 at a magnification of 10K;

[0027] Figure 4 This is a scanning electron microscope image of the sodium ion battery positive electrode material prepared in Comparative Example 2 at a magnification of 10K. DETAILED DESCRIPTION

[0028] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific implementation methods or embodiments and are not intended to limit the present invention.

[0030] The present invention provides a sodium ion battery positive electrode material, the chemical general formula of the sodium ion battery positive electrode material is Na a Li g Ni b Fe c Mn d A e Co f O2, wherein 1.05≤a≤1.15, 0.2≤b≤0.4, 0.2≤c≤0.4, 0.2≤d≤0.4, 0.0001≤e≤0.005, 0.0002≤f≤0.004, 0.02≤g≤0.2, and a / (b+c+d) is 1.05-1.15, A is an element with an ionic radius greater than or equal to 0.080nm, and the Na-O interlayer spacing is 3.00Å-3.16Å.

[0031] It should be noted that the molar ratio of sodium element to nickel, iron and manganese elements in the sodium ion battery positive electrode material, a / (b+c+d), is the sodium ratio of the sodium ion battery positive electrode material. The sodium content in the sodium ion battery positive electrode material can be evaluated by the sodium ratio based on the molar amount of nickel, iron and manganese elements in the sodium ion battery positive electrode material.

[0032] The sodium ion battery positive electrode material of the present invention has a sodium ratio of 1.05-1.15 and a Na-O interlayer spacing of 3.00Å-3.16Å, and the grain boundary is enriched with A elements with an ion radius greater than or equal to 0.080nm. On the one hand, it overcomes the technical difficulties such as excessive alkali content caused by traditional high sodium content and thus low rate, so that the sodium ion battery positive electrode material has both high sodium ratio and low residual alkali content, thereby improving the rate and cycle stability of the sodium ion battery positive electrode material; on the other hand, the sodium ions in the sodium ion battery positive electrode material are easy to be deintercalated, which is beneficial to improve the capacity, and the synergistic effect between the elements in the sodium ion battery positive electrode material is not only beneficial to further improve the rate, but also improve the interface electronic conductivity, which is beneficial to reduce the resistance.

[0033] In one embodiment, a / (b+c+d) includes but is not limited to any one of 1.05, 1.06, 1.07, 1.08, 1.09, 1.10, 1.11, 1.12, 1.13, 1.14, and 1.15, or a range of values ​​between any two of them, preferably 1.06-1.14.

[0034] It can be understood that when b+c+d=1, the sodium ratio of the sodium ion battery positive electrode material is the value a.

[0035] The A element with an ion radius greater than or equal to 0.080nm is enriched at the grain boundary to form an alloy phase, which is beneficial to lowering the melting point and improving the crystallinity of the positive electrode material of the sodium ion battery. It can not only cooperate with the sodium-rich structure and increase the sodium ratio, but also help to increase the Na-O layer spacing, making it easier for sodium ions to be deintercalated, thereby improving the capacity and rate of the positive electrode material of the sodium ion battery.

[0036] In one embodiment, the A element includes but is not limited to at least one of Sr, Y, K, Ca, Ce, and Rb, preferably Sr.

[0037] Preferably, 1.08≤a≤1.12, and / or 0.25≤b≤0.35, and / or 0.25≤c≤0.35, and / or 0.25≤d≤0.35, and / or 0.001≤e≤0.004, and / or 0.0003≤f≤0.001, and / or 0.05≤g≤0.12.

[0038] In one embodiment, the sodium ion battery positive electrode material has a layered structure, and Co is distributed on the surface of the sodium ion battery positive electrode material, which is beneficial to further reduce the amount of residual alkali on the surface.

[0039] Therefore, the sodium ion battery positive electrode material of the present invention has excellent high-rate performance and cycle stability, and has high capacity and low resistance. When used in sodium ion batteries under the condition of a charge and discharge rate of 5C, the voltage drop is as low as within 6.5%, thereby improving the application advantages of sodium ion batteries.

[0040] The present invention provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising:

[0041] S1, according to Na a Li g Ni b Fe c Mn d A e Co fO2, wherein 1.05≤a≤1.15, 0.2≤b≤0.4, 0.2≤c≤0.4, 0.2≤d≤0.4, 0.0001≤e≤0.005, 0.0002≤f≤0.004, 0.02≤g≤0.2, and a / (b+c+d) is a ratio of 1.05-1.15, a nickel iron manganese hydroxide precursor, a sodium source, a lithium source and a compound containing an element A are mixed and sintered once to obtain a pre-product, A is an element having an ion radius greater than 0.080 nm, and the sodium source includes a first sodium source having a melting point less than or equal to 350° C., and the molar fraction of the first sodium source in the sodium source is 1.5%-20%;

[0042] S2, mixing the pre-product with a cobalt source and performing secondary sintering to obtain the sodium ion battery positive electrode material.

[0043] In the preparation process of traditional sodium ion battery positive electrode materials, a high sodium ratio will inevitably cause a high amount of surface alkali, which not only leads to a low rate of sodium ion battery positive electrode materials, but also makes the processing performance and kinetic performance of sodium ion battery positive electrode materials worse. The present invention introduces a specific content of low melting point sodium source as a composite sodium source, and cooperates with a specific amount of lithium source, nickel iron manganese hydroxide precursor and A element-containing compound for primary sintering to improve the uniformity of sintering and the crystallinity of the sintered pre-product, so that the sodium ion battery positive electrode material has a high sodium ratio and a low residual alkali content at the same time, thereby improving the rate and cycle stability of the sodium ion battery positive electrode material. Then, a cobalt source is used for secondary sintering to further increase the rate, improve the interface electronic conductivity, and reduce resistance.

[0044] In step S1, the first sodium source includes but is not limited to at least one of sodium oxalate, sodium acetate, sodium bicarbonate, and sodium nitrate, preferably sodium oxalate.

[0045] In one embodiment, the sodium source further includes a second sodium source having a melting point greater than or equal to 800° C., wherein the second sodium source includes but is not limited to at least one of sodium carbonate, sodium oxide, sodium chloride, and sodium sulfate, preferably sodium carbonate.

[0046] Preferably, the molar ratio of sodium ions in the second sodium source to sodium ions in the first sodium source is 5:1-50:1, and more preferably 5:1-20:1. The mutual coordination of the first sodium source and the second sodium source is conducive to avoiding the problem of increased alkali content caused by the decomposition of the first sodium source to produce carbon dioxide, making the sintering more complete, thereby further increasing the interlayer spacing.

[0047] In one embodiment, the lithium source includes but is not limited to at least one of lithium carbonate, lithium hydroxide, and lithium oxalate, preferably lithium carbonate.

[0048] In one embodiment, the A element includes but is not limited to at least one of Sr, Y, K, Ca, Ce, and Rb, preferably Sr.

[0049] In one embodiment, the primary sintering is performed at a temperature of 880° C. to 980° C. for a time of 6 h to 14 h.

[0050] In step S2, the pre-product is preferably crushed before the secondary sintering to reduce the particle size of the pre-product, which is beneficial to improving the secondary sintering effect, thereby further reducing the residual alkali on the surface of the sodium ion battery positive electrode material.

[0051] In one embodiment, the secondary sintering is performed at a temperature of 700° C. to 900° C. for a time of 6 h to 14 h.

[0052] The present invention provides a positive electrode sheet, comprising the above-mentioned positive electrode material for a sodium ion battery.

[0053] Specifically, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, and the positive electrode film layer includes the positive electrode material described in the present invention.

[0054] In one embodiment, the positive electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, aluminum foil may be used. The composite current collector includes a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material on a polymer material substrate. Optionally, the metal material includes but is not limited to one or more of aluminum, aluminum gold, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. Optionally, the polymer material substrate includes but is not limited to one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0055] In one embodiment, the positive electrode film layer is mainly composed of the positive electrode material described in the present invention, a binder and a conductive agent. Optionally, the conductive agent includes but is not limited to at least one of carbon black, carbon dots, carbon nanotubes, graphene and carbon nanofibers, wherein the carbon black includes superconducting carbon, acetylene black or Ketjen black.

[0056] It should be noted that the present invention does not limit the preparation method of the positive electrode sheet, and the positive electrode sheet can be prepared by conventional processes, for example: the positive electrode material, the conductive agent, the binder and any other components are dispersed in a solvent to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and the positive electrode sheet can be obtained after drying, cold pressing and other processes. Optionally, the solvent includes but is not limited to N-methylpyrrolidone.

[0057] The present invention provides a sodium ion battery, comprising the positive electrode sheet as described above.

[0058] The sodium ion battery is mainly composed of a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet, the separator and the electrolyte can adopt any conventional commercially available negative electrode sheet (or negative electrode material), the separator and the electrolyte, and the present invention is not limited to this.

[0059] The present invention also provides an electrical device, comprising the sodium ion battery as described above.

[0060] It is understandable that the above-mentioned power consumption settings include any equipment using the above-mentioned sodium ion batteries, such as electric vehicles, power tools, electronic products, energy storage systems, and office equipment, but are not limited thereto.

[0061] Hereinafter, the sodium ion battery positive electrode material, preparation method and application thereof will be further described by the following specific examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0062] Example 1

[0063] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, and the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0064] Example 2

[0065] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33(OH)2 precursor, 5.80kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0066] Example 3

[0067] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.28kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0068] Example 4

[0069] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33(OH)2 precursor, 6.52kg of sodium carbonate, 0.152kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and the mixture was stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a positive electrode material for a sodium ion battery.

[0070] Example 5

[0071] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 5.43kg of sodium carbonate, 1.52kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and the mixture was stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0072] Example 6

[0073] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33(OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, 0.09kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0074] Example 7

[0075] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, 0.94kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0076] Example 8

[0077] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33(OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for sintering at a temperature of 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 3.6g of Co(OH)3 was added, and the mixture was stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for sintering at a temperature of 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a positive electrode material for a sodium ion battery.

[0078] Example 9

[0079] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 18g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0080] Example 10

[0081] Add 10kg of Ni into a 50L high-speed mixer. 28 Fe 35 Mn 37(OH)2 precursor, 8.09kg of sodium sulfate, 0.96kg of sodium bicarbonate, 0.47kg of lithium hydroxide and 12.5g of Y2O3 were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 940℃ at a rate of 5℃ / min for heat preservation and sintering for 12h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm for 12min in a 20L high mixer, then placed in a sagger, introduced into an air atmosphere, heated to 780℃ at a rate of 5℃ / min for heat preservation and sintering for 9h, then cooled with the furnace, and the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0082] Embodiment 11

[0083] Add 10kg of Ni into a 50L high-speed mixer. 35 Fe 26 Mn 39 (OH)2 precursor, 4.68kg of sodium oxide, 1.24kg of sodium acetate, 1.23kg of lithium acetate and 50g of CeO2 were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 900℃ at a rate of 5℃ / min for heat preservation and sintering for 9h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm for 12min in a 20L high mixer, then placed in a sagger, introduced into an air atmosphere, heated to 750℃ at a rate of 5℃ / min for heat preservation and sintering for 11h, then cooled with the furnace, and the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0084] Comparative Example 1

[0085] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33(OH)2 precursor, 5.56kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0086] Comparative Example 2

[0087] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.64kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0088] Comparative Example 3

[0089] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.64kg of sodium carbonate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0090] Comparative Example 4

[0091] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 3.65kg of sodium carbonate, 3.8kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a positive electrode material for a sodium ion battery.

[0092] Comparative Example 5

[0093] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a positive electrode material for a sodium ion battery.

[0094] Comparative Example 6

[0095] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33(OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, 2.35kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and the mixture was stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a positive electrode material for a sodium ion battery.

[0096] Comparative Example 7

[0097] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, and 0.47kg of lithium carbonate were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, and then cooled with the furnace. The materials after being taken out of the furnace were crushed and sieved with a jet mill, and 9g of Co(OH)3 was added. The mixture was stirred and mixed at 800rpm in a 20L high mixer for 12min, and then placed in a sagger, introduced into an air atmosphere, and heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h. Then, the materials after being taken out of the furnace were crushed and sieved with a jet mill to obtain a positive electrode material for a sodium ion battery.

[0098] Comparative Example 8

[0099] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 33g of MgO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 9g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, and the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0100] Comparative Example 9

[0101] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0102] Comparative Example 10

[0103] Add 10kg of Ni into a 50L high-speed mixer. 0.33 Fe 0.33 Mn 0.33 (OH)2 precursor, 6.04kg of sodium carbonate, 0.76kg of sodium oxalate, 0.47kg of lithium carbonate and 24g of SrO were stirred and mixed at 800rpm for 12min to obtain a mixture. The mixture was placed in a sagger, introduced into an air atmosphere, heated to 920℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill, 90g of Co(OH)3 was added, and stirred and mixed at 800rpm in a 20L high mixer for 12min, then placed in a sagger, introduced into an air atmosphere, heated to 800℃ at a rate of 5℃ / min for heat preservation and sintering for 10h, then cooled with the furnace, the material after being taken out of the furnace was crushed and sieved with a jet mill to obtain a sodium ion battery positive electrode material.

[0104] Among them, the raw material ratios and product ratios used in the preparation of Examples 1 to 11 and Comparative Examples 1 to 10 are shown in Table 1.

[0105] Table 1

[0106]

[0107] The sodium ion battery positive electrode material prepared in Example 1 was subjected to cross-section EDS testing. The testing method was as follows: 0.2 g of the material to be tested was placed in an ion milling Gatan 697 Ilion II. The material to be tested was pre-treated first, the high-purity Ar outlet pressure was 0.18 MPa, and the current of the left and right guns was controlled to be less than 6 μA at 5 keV. After the pre-treatment, the test was performed, the angles of the left and right guns were 0 degrees, and the ion beam energy was 5 keV for cross-sectioning. After cross-sectioning, SEM observation and EDS measurement analysis were performed using Hitachi Regulus 8100. The results are as follows: Figure 1 As shown, it can be seen that Co is mainly distributed on the surface of the sodium ion battery positive electrode material.

[0108] The sodium ion battery positive electrode materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 were subjected to morphological tests under 10K magnification conditions, and the results were as follows: Figure 2 , Figure 3 as well as Figure 4 And embodiment 1 to embodiment 11 and comparative example 1 to comparative example 10 were characterized and tested, and the results are shown in Table 2.

[0109] The sodium ion battery positive electrode materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 were assembled into button cells. The specific method was as follows: the prepared sodium ion battery positive electrode material, acetylene black and polyvinylidene fluoride (PVDF) were weighed in a mass ratio of 90:5:5, mixed evenly, added with NMP and stirred for 2 hours to form a viscous slurry, evenly coated on an aluminum foil, vacuum baked at 80°C, pressed into sheets, and cut into positive electrode sheets with a diameter of 14 mm; a pure sodium sheet with a diameter of 16 mm was used as a negative electrode sheet, Tianci ENA-18 was used as an electrolyte, and a PP / PE / PP composite separator was used, and the button cells were assembled in a glove box filled with argon. The performance test results are shown in Table 3.

[0110] Test methods include:

[0111] (1) Water measurement of CO3 2- : Weigh 2g of the material to be tested, add 100mL of pure water, stir for 30min, filter about 50mL with filter paper, transfer 10mL, use 0.05mol / L HCl solution, and determine the endpoint according to the potentiometric titration to obtain CO3 2- content;

[0112] (2) Ethanol OH measurement - : Weigh 2g of the material to be tested, add 100mL of pure water, stir for 60min, filter about 50mL with filter paper, transfer 10mL, use 0.05mol / L HCl solution, and determine the endpoint according to the potentiometric titration to obtain OH - content;

[0113] (3) Powder resistance detection method: Use PD-51 test equipment, MCP-T700 impedance meter, and four-probe method. Weigh 4g of the material to be tested and place it in a measuring cylinder with a radius of 10mm. Record the powder resistance value under a pressure of 12MPa.

[0114] (4) Detection method of Na-O interlayer spacing at 10% state of charge (SOC): discharge the button battery to 10% SOC, and perform XRD test on the corresponding positive electrode using Bruker's XRD diffractometer. The data is processed using Bruker's commercial software TOPAS. The operation process of XRD data processing to obtain unit cell parameters: import the matching CIF file into TOPAS, change and confirm the atomic position, element type and temperature factor of the imported structure file, select the unit cell parameters a and c for fitting, and then obtain the Na-O interlayer spacing;

[0115] (5) 0.1C capacity detection method: Put the assembled button cell in the blue electricity equipment, test temperature 25±1℃, test voltage 2.0~4.0V, 0.1C / 0.1C charge-discharge, charge cut-off current is 0.05C (1C nominal capacity 130mAh / g), get 0.1C discharge capacity, then discharge at 5C to get 5C discharge capacity;

[0116] (6) Detection method of average voltage drop at 5C: Measure the energy density and discharge capacity at 0.1C, and obtain V1 according to energy density / discharge capacity; Measure the energy density and discharge capacity at 5C, and obtain V2 according to energy density / discharge capacity; Then calculate the average voltage drop according to (V1-V2) / V1×100%;

[0117] (7) Method for testing the capacity retention rate after 50 cycles: The battery was a Xinwei CT3008-5V3A-A1 battery, with a cycle voltage of 4~2V and a constant voltage cutoff current of 20mA at 25°C for 50 cycles.

[0118] Table 2

[0119]

[0120] Table 3

[0121]

[0122] according to Figures 2 to 4As shown in Tables 1 to 3, compared with Example 1, due to the low sodium ratio in Comparative Example 1, the alkali content is low, but the Na-O interlayer spacing is small, the effective sodium is less, resulting in reduced capacity and rate, and the primary particle size is reduced, which is easier to agglomerate, and the compaction density is reduced, resulting in a further reduction in capacity. Comparison of Example 1 with Comparative Example 2 shows that due to the high sodium ratio in Comparative Example 2, there is a significant amount of alkali on the surface, which affects the capacity and rate.

[0123] By comparing Example 1 with Comparative Example 3, it can be seen that only using high-melting-point sodium carbonate for sintering will cause insufficient sintering, resulting in high alkali content and powder resistance, small Na-O interlayer spacing, and low capacity; by comparing Example 1 with Comparative Example 4, it can be seen that the proportion of sodium oxalate is too high, resulting in increased alkali content and powder resistance, excessively large Na-O interlayer spacing, and significantly reduced capacity.

[0124] By comparing Example 1 with Comparative Example 5, it can be seen that the lack of lithium element leads to an increase in the alkali content and powder resistance, and the capacity and rate performance are significantly reduced; by comparing Example 1 with Comparative Example 6, it can be seen that there is too much lithium element, which leads to a high alkali content and powder resistance, and the capacity and rate performance are significantly deteriorated.

[0125] By comparing Example 1 with Comparative Example 7, it can be seen that the lack of doping elements with a specific ionic radius leads to a significant decrease in the Na-O interlayer spacing, poor crystallinity, increased alkali content, and reduced capacity; by comparing Example 1 with Comparative Example 8, it can be seen that the use of magnesium with a smaller ionic radius as a doping element also leads to poor crystallinity, increased powder resistance and alkali content, and deterioration of capacity and rate.

[0126] By comparing Example 1 with Comparative Example 9, it can be seen that the lack of cobalt coating leads to a significant increase in the alkali content and deterioration of the rate performance; by comparing Example 1 with Comparative Example 10, it can be seen that excessive cobalt coating, although the alkali content is reduced, the internal sodium precipitation causes a decrease in capacity and deteriorates the rate performance.

[0127] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0128] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A sodium ion battery positive electrode material, characterized in that: The chemical formula of the sodium ion battery positive electrode material is Na a Li g Ni b Fe c Mn d A e Co f O2, wherein 1.05≤a≤1.15, 0.2≤b≤0.4, 0.2≤c≤0.4, 0.2≤d≤0.4, 0.0001≤e≤0.005, 0.0002≤f≤0.004, 0.02≤g≤0.2, and a / (b+c+d) is 1.05-1.15, A is an element having an ion radius greater than or equal to 0.080nm, the A element is selected from at least one of Sr, Y, K, Ca, Ce, and Rb, and the Na-O interlayer spacing is 3.00Å-3.16Å at 10% charge state.

2. The sodium ion battery positive electrode material according to claim 1, characterized in that a / (b+c+d) is 1.06-1.

14.

3. The sodium ion battery positive electrode material according to claim 1, characterized in that The sodium ion battery positive electrode material is a layered structure, and Co is distributed on the surface of the sodium ion battery positive electrode material.

4. A method for preparing a positive electrode material for a sodium ion battery according to any one of claims 1 to 3, characterized in that: include: According to Na a Li g Ni b Fe c Mn d A e Co f O2, 1.05≤a≤1.15, 0.2≤b≤0.4, 0.2≤c≤0.4, 0.2≤d≤0.4, 0.0001≤e≤0.005, 0.0002≤f≤0.004, 0.02≤g≤0.2, and a / (b+c+d) is a ratio of 1.05-1.15, mixing a nickel iron manganese hydroxide precursor, a sodium source, a lithium source and a compound containing an element A for one sintering to obtain a pre-product, A is an element having an ion radius greater than 0.080nm, and the element A is selected from at least one of Sr, Y, K, Ca, Ce, and Rb, and the sodium source includes a first sodium source having a melting point less than or equal to 350°C, and a second sodium source having a melting point greater than or equal to 800°C, and the molar fraction of the first sodium source in the sodium source is 1.5%-20%; The pre-product is mixed with a cobalt source and subjected to secondary sintering to obtain the sodium ion battery positive electrode material.

5. The method for preparing a positive electrode material for a sodium ion battery according to claim 4, characterized in that: The first sodium source is selected from at least one of sodium oxalate, sodium acetate, sodium bicarbonate and sodium nitrate.

6. The method for preparing a positive electrode material for a sodium ion battery according to claim 4, characterized in that: The second sodium source is selected from at least one of sodium carbonate, sodium oxide, sodium chloride and sodium sulfate.

7. The method for preparing a positive electrode material for a sodium ion battery according to claim 6, characterized in that: The molar ratio of sodium ions in the second sodium source to sodium ions in the first sodium source is 5:1-50:

1.

8. The method for preparing a positive electrode material for a sodium ion battery according to claim 4, characterized in that: The lithium source is selected from at least one of lithium carbonate, lithium hydroxide and lithium oxalate.

9. The method for preparing a positive electrode material for a sodium ion battery according to claim 4, characterized in that: The primary sintering temperature is 880°C-980°C and the time is 6h-14h; And / or, the secondary sintering is carried out at a temperature of 700° C.-900° C. and for a time of 6 h-14 h.

10. A positive electrode sheet, characterized in that: The invention comprises a sodium ion battery positive electrode material as claimed in any one of claims 1 to 3.

11. A sodium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 10.

12. An electrical device, characterized in that: Comprising the sodium ion battery as claimed in claim 11.

Citation Information

Patent Citations

  • Sodium-ion battery positive electrode material and preparation method thereof

    CN116706017A

  • Sodium-ion battery positive electrode material and preparation method thereof

    CN117239081A