Hetero-element doped porous silicon nitride material and preparation method and application thereof
The preparation of heteroelement-doped porous silicon nitride materials solves the problems of small surface area and limited properties of silicon nitride in catalytic reactions, significantly improves its catalytic activity and stability in acetylene selective hydrogenation reactions, and achieves Highly efficient catalytic effect.
Patent Information
- Application Number
- CN202410905709.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-08
AI Technical Summary
Existing silicon nitride has a small surface area and limited surface properties in catalytic reactions, resulting in insufficient reliability and activity in catalytic reactions, especially poor performance in acetylene selective hydrogenation reactions.
A method for preparing heteroelement-doped porous silicon nitride materials is adopted. By mixing phosphorus-, sulfur-, and boron-containing precursors with silicon nitride in a solvent, and subjecting them to microwave heating and high-temperature treatment, a heteroelement-doped porous silicon nitride material with a porous structure is formed. Heteroporous silicon nitride material is used as a catalyst for the selective hydrogenation of acetylene.
The surface area and active sites of silicon nitride are significantly increased, and its catalytic activity and stability in the selective hydrogenation reaction of acetylene are enhanced. The acetylene conversion rate can reach more than 92.5%, and the ethylene selectivity can reach more than 99%.
Smart Images

Figure CN118458709B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a silicon nitride material and a preparation method and application thereof. Background Art
[0002] Silicon nitride (Si3N4) belongs to the hexagonal system and can be divided into two crystal forms: α-Si3N4 and β-Si3N4. Si3N4 has the advantages of good mechanical strength and thermal conductivity, stable chemical properties, low thermal expansion coefficient, high hardness and relative inertness. In the field of high-temperature materials, it has excellent properties such as oxidation resistance, corrosion resistance and thermal shock resistance. Its cost is relatively low, and its separation efficiency (especially for particles in the range of 0.1 to 100μm) is high and it has biocompatibility, which has attracted more and more attention. Si3N4 is widely used in the field of ceramics to manufacture high-performance ceramic products; in the electronics industry, it can be used as a heat dissipation material and insulating parts; in the field of mechanical manufacturing, it is often used for wear-resistant parts; in the metallurgical industry, it can also be used as a refractory material. In addition, these excellent properties of Si3N4 make it have extremely high application value in the fields of national defense and military industry, semiconductor thermal conductive substrates, biomedicine and new technologies.
[0003] Commercial silicon nitride is usually composed of low-temperature (1200°C) α-Si3N4 or high-temperature (1500°C) β-Si3N4, produced by grinding the body ceramic to produce a low specific surface area (usually less than 10 m 2 / g) of powder, which may limit the catalyst loading and the number of active sites. In addition, pure Si3N4 has limited surface properties and weak interaction with catalysts, which makes the reliability of pure silicon nitride in catalytic reactions unguaranteed. Therefore, improving its reliability has always been an important direction of Si3N4 research.
[0004] At present, silicon nitride is generally used as a catalyst carrier in the field of catalysis. CN 116273136 A discloses a Cu / silicon nitride catalyst and its preparation method and its application in CO catalytic oxidation. CN 114433246 A discloses a silicon nitride carrier with a high specific surface area and its preparation method, the silicon nitride carrier is used to prepare a highly dispersed transition metal catalyst anchored to silicon nitride, and the catalyst is used in the CO hydrogenation to alcohol reaction. However, there is no report on the application of silicon nitride in the selective hydrogenation reaction of acetylene.
[0005] Based on the above background, it is necessary to develop a method for preparing Si3N4 doped with heteroelements, modify Si3N4, increase its specific surface area and surface active sites, and improve its activity and stability in catalytic reactions, especially in the selective hydrogenation of acetylene. Summary of the invention
[0006] The first problem to be solved by the present invention is to overcome the problems of low specific surface area and limited surface properties of pure Si3N4 currently used in catalytic reactions, and to provide a method for preparing a porous silicon nitride material doped with hetero-elements.
[0007] The second problem to be solved by the present invention is to provide a porous silicon nitride material doped with heteroelement to increase its specific surface area and surface active sites.
[0008] The third problem to be solved by the present invention is to provide the use of the heteroelement-doped porous silicon nitride material as a catalyst in the selective hydrogenation reaction of acetylene, which has high catalytic activity and high stability.
[0009] The technical solution adopted by the present invention is described in detail below.
[0010] In a first aspect, the present invention provides a method for preparing a heteroelement-doped porous silicon nitride material, comprising the following steps:
[0011] 1) fully mixing a phosphorus-containing precursor, a sulfur-containing precursor, a boron-containing precursor, silicon nitride and a solvent, and stirring to obtain a mixture; the feeding ratio of the phosphorus-containing precursor, the sulfur-containing precursor, the boron-containing precursor and the silicon nitride is according to the element molar ratio of phosphorus: sulfur: boron: nitrogen = 0.1~1: 0.1~1: 0.1~1: 0.5~5, where the mole number of phosphorus is the total mole number of phosphorus contained in the four types of substances, namely, the phosphorus-containing precursor, the sulfur-containing precursor, the boron-containing precursor and the silicon nitride, and the mole numbers of sulfur, boron and nitrogen are also calculated in the above manner;
[0012] 2) allowing the mixture obtained in step 1) to stand to obtain a gel-like substance;
[0013] 3) subjecting the gel-like substance obtained in step 2) to microwave heating and drying;
[0014] 4) subjecting the mixture after the drying treatment in step 3) to high temperature treatment using a Joule heating apparatus;
[0015] 5) Cooling the mixture after high temperature treatment in step 4) to room temperature, and then washing, drying and grinding to obtain the impurity-doped porous silicon nitride material.
[0016] Furthermore, the phosphorus-containing precursor in step 1) is selected from one or more of hydroxyethylidene diphosphonic acid, (2-hydroxyethyl)phenylphosphonic acid, tetraphenylphosphine chloride, ethyl dichlorophosphate, pyrophosphoric acid, methyldiphenylphosphine oxide, metaphosphoric acid, triphenylphosphine sulfide and methyltriphenylphosphine chloride.
[0017] Furthermore, the sulfur-containing precursor in step 1) is selected from one or more of diphenyl sulfoxide, diphenylthiourea, dithiobenzoic acid, 2-thiophenecarboxylic acid, sodium diethyldithiocarbamate, diphenyl disulfide, benzothiazole and 2-aminobenzothiazole.
[0018] Furthermore, the boron-containing precursor in step 1) is selected from one or more of boric acid, trimethyl borate, triethyl borate, phenylboric acid, p-hydroxyphenylboric acid, p-methylphenylboric acid and boron oxide.
[0019] Furthermore, the silicon nitride in step 1) is selected from commercially available silicon nitride.
[0020] Furthermore, the solvent in step 1) is selected from at least one of water, methanol, ethanol, acetone, sucrose aqueous solution, and starch aqueous solution.
[0021] Furthermore, in step 1), the mass volume ratio of the silicon nitride to the solvent is 1-5 g: 5-15 mL.
[0022] Furthermore, the stirring time in step 1) is 1-3 h.
[0023] Furthermore, in step 2), the mixture is allowed to stand at a temperature of room temperature to 90° C. for a period of 0.5 to 3 h.
[0024] Furthermore, in step 3), the drying temperature is 60-150° C., the vacuum degree is 100-100000 Pa, and the drying time is 2-20 h.
[0025] Furthermore, in step 4), the temperature of the high temperature treatment is 300-1800° C.; the time of the high temperature treatment is 1-30 hours; and the atmosphere of the high temperature treatment is an inert atmosphere, specifically helium, argon or nitrogen.
[0026] Furthermore, in step 5), the washing solvent is selected from deionized water, hydrogen peroxide, methanol, ethanol, propanol, cyclohexanol, butanol, acetone, liquid ammonia or aqueous ammonia.
[0027] Furthermore, the drying temperature in step 5) is 100-120° C., and the drying time is 10-15 hours.
[0028] Furthermore, the dried compound in step 5) is ground into a powder of 10-200 mesh, and can be briquetteed into different particle sizes according to needs.
[0029] In a second aspect, the present invention provides an impurity-doped porous silicon nitride material prepared according to the preparation method described in the first aspect.
[0030] The heteroelement-doped silicon nitride material is mainly composed of a porous silicon nitride material, which contains a small amount of carbon, phosphorus, oxygen and boron elements. Preferably, the molar ratio of nitrogen to silicon in the silicon nitride material is 4:3. The porous silicon nitride carrier has a variety of microstructures, and the microscopic morphology of the prepared catalyst is different according to the selection of different precursors and solvents.
[0031] In a third aspect, the present invention provides the use of the heteroelement-doped porous silicon nitride material described in the second aspect as a catalyst in the selective hydrogenation reaction of acetylene.
[0032] The acetylene selective hydrogenation synthesis reaction is specifically implemented as follows: in a fixed bed reactor, the impurity element doped porous silicon nitride material is loaded, a raw gas is introduced, the raw gas includes hydrogen and acetylene, the reaction temperature is set to 150-300° C., and the reaction pressure is set to 0.1-0.5 MPa, and ethylene is generated by the reaction.
[0033] Furthermore, the ratio of the amount of hydrogen and acetylene in the raw gas is n(H2) / n(C2H2) = 0.8~1.2 / 1. The acetylene gas space velocity is 30~370h -1 .
[0034] The heteroelement-doped porous silicon nitride catalyst of the present invention has good reaction activity in the above-mentioned acetylene hydrogenation reaction, and the acetylene conversion rate can reach up to more than 92.5%, and the ethylene selectivity can reach up to more than 99%.
[0035] Compared with the prior art, the beneficial effects of the present invention are:
[0036] (1) The impurity-doped porous silicon nitride material of the present invention can controllably adjust the physicochemical properties of the material by adjusting the doping raw materials, Si3N4 and solvent during the preparation process; microwave oven heating is used in the preparation process, which is energy-saving and efficient, with uniform heating, simple operation, easy controllable conditions, and helps to obtain high-purity products, thereby expanding its application range; Joule heating apparatus is used in the preparation process to perform high-temperature treatment on the material, which has the advantages of rapid response, high repeatability, precise control, clean and environmental protection, high energy utilization rate and good stability.
[0037] (2) The heteroelement-doped porous silicon nitride material prepared by the present invention has many advantages. It can not only significantly increase the surface area of silicon nitride, but also increase the active sites. It has low production cost, little harm to the environment, and has high research value.
[0038] (3) The heteroelement-doped porous Si3N4 material prepared by the present invention has excellent activity itself and can be directly used as a catalyst. It exhibits high catalytic activity in the selective hydrogenation reaction of acetylene, with the acetylene conversion rate reaching up to more than 92.5% and the ethylene selectivity reaching up to more than 99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 SEM image of the material obtained in Comparative Example 7;
[0040] Figure 2 is a SEM image of the material prepared in Example 10;
[0041] Figure 3 This is the long-term operation data of the heteroelement-doped porous silicon nitride catalyst prepared in Example 5. DETAILED DESCRIPTION
[0042] The present invention is described below with specific examples. It is necessary to point out that the examples are only used to further illustrate the present invention, but cannot be understood as limiting the scope of protection of the present invention, and the present invention is not limited thereto in any way. Those skilled in the art in this field can make some non-essential improvements and adjustments based on the content of the above invention.
[0043] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained by conventional technical means or purchased commercially.
[0044] Example 1
[0045] (1) Weigh 5.15 g of hydroxyethylidene diphosphonic acid, 9.1 g of diphenyl sulfoxide, 3.1 g of boric acid, and 7 g of silicon nitride, add 10 ml of deionized water, and stir for 2 h to mix thoroughly;
[0046] (2) placing the mixture at 60°C for 1 hour to turn it into a gel-like substance;
[0047] (3) subjecting the gel-like substance to microwave heating and drying at 110° C. and 10,000 Pa for 2 h;
[0048] (4) The dried mixture was heated at 10 °C min under a nitrogen atmosphere. -1 The heating rate was raised to 1100°C and high temperature treatment was carried out using a Joule heating apparatus for 4 h;
[0049] (5) cooling the treated catalyst to room temperature and washing it three times with deionized water;
[0050] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0051] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 220°C, acetylene space velocity 120h -1, the volume ratio of hydrogen to acetylene was 1:1.2. The reaction conversion rate was 63% and the selectivity of vinyl chloride was 99%.
[0052] Example 2
[0053] (1) Weigh 13.17 g of tetraphenylphosphine chloride, 3.458 g of dithiobenzoic acid, 4.71 g of trimethyl borate, and 4.2 g of silicon nitride, add 12 ml of deionized water, and stir for 1.5 h to mix thoroughly;
[0054] (2) placing the mixture at 90° C. and leaving it to stand for 0.5 h to turn it into a gel-like substance;
[0055] (3) subjecting the gel-like substance to microwave heating and drying at 80° C. and 1000 Pa for 12 h;
[0056] (4) subjecting the dried mixture to high temperature treatment at 1300° C. for 2.5 h using a Joule heater in a helium atmosphere;
[0057] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with ethanol;
[0058] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 30 mesh;
[0059] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 200 °C, acetylene space velocity 100 h -1 , the volume ratio of hydrogen to acetylene was 1:1; the reaction conversion rate was 92% and the ethylene selectivity was 99%.
[0060] Example 3
[0061] (1) Weigh 8 g of hydroxyethylidene diphosphonic acid, 5.58 g of sodium diethyldithiocarbamate, 11.39 g of triethyl borate, and 2.73 g of silicon nitride, add 8 ml of methanol, and stir for 1.5 h to mix thoroughly;
[0062] (2) leaving the mixture at room temperature for 3 hours to turn it into a gel-like substance;
[0063] (3) subjecting the gel-like substance to microwave heating and drying at 60° C. and 5000 Pa for 10 h;
[0064] (4) subjecting the dried mixture to high temperature treatment at 300° C. for 4 h using a Joule heater under an argon atmosphere;
[0065] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with methanol;
[0066] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 50 mesh;
[0067] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 180°C, acetylene space velocity 30h -1 , the volume ratio of hydrogen to acetylene was 0.8:1; the reaction conversion rate was 90% and the ethylene selectivity was 97%.
[0068] Example 4
[0069] (1) Weigh 8.72 g of ethyl dichlorophosphate, 5.76 g of 2-thiophenecarboxylic acid, 4.88 g of phenylboric acid, and 5.2 g of silicon nitride, add 15 ml of acetone, and stir for 1.5 h to mix thoroughly;
[0070] (2) placing the mixture at 70° C. for 2 h to turn it into a gel-like substance;
[0071] (3) subjecting the gel-like substance to microwave heating and drying at 120° C. and 2000 Pa for 15 h;
[0072] (4) subjecting the dried mixture to high temperature treatment at 800° C. for 14 h using a Joule heater under a nitrogen atmosphere;
[0073] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with hydrogen peroxide;
[0074] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 10 mesh;
[0075] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 200 °C, acetylene space velocity 150 h -1 , the volume ratio of hydrogen to acetylene was 1:1; the reaction conversion rate was 75% and the ethylene selectivity was 98%.
[0076] Example 5
[0077] (1) Weigh 6.4 g of metaphosphoric acid, 9.52 g of diphenyl disulfide, 12.06 g of p-hydroxyphenylboric acid, and 4.6 g of silicon nitride, add 15 ml of deionized water, and stir for 1.5 h to mix thoroughly;
[0078] (2) placing the mixture at 90° C. for 1 h to turn it into a gel-like substance;
[0079] (3) subjecting the gel-like substance to microwave heating and drying treatment at 150° C. and 10,000 Pa for 11 h;
[0080] (4) subjecting the dried mixture to high temperature treatment at 300° C. for 18 h using a Joule heater under an argon atmosphere;
[0081] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with cyclohexanol;
[0082] (6) The washed catalyst was subjected to microwave heating, dried at 110° C. for 12 hours, and ground to a particle size of 80 mesh;
[0083] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 170°C, acetylene space velocity 200h -1 , the volume ratio of hydrogen to acetylene was 1.2:1; the reaction conversion rate was 96% and the ethylene selectivity was 99%. The long-term operation data of the catalyst can be found in Figure 3 During the nearly 60 hours of operation, the catalyst maintained high catalytic activity (acetylene conversion greater than 96%) and selectivity (ethylene selectivity greater than 99%), and no obvious deactivation occurred during the reaction.
[0084] Example 6
[0085] (1) Weigh 13.32 g of pyrophosphoric acid, 9.24 g of dithiobenzoic acid, 4.1772 g of boron oxide, and 5 g of silicon nitride, add 15 ml of a 20% sucrose aqueous solution, and stir for 1.5 h to mix thoroughly;
[0086] (2) placing the mixture at 50° C. for 2.5 h to turn it into a gel-like substance;
[0087] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 8000 Pa for 20 h;
[0088] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater under an argon atmosphere;
[0089] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it with liquid ammonia three times;
[0090] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0091] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 300 °C, acetylene space velocity 300 h -1 , the volume ratio of hydrogen to acetylene was 1:1; the reaction conversion rate was 95% and the ethylene selectivity was 99%.
[0092] Example 7
[0093] (1) Weigh 13.32 g of (2-hydroxyethyl)phenylphosphonic acid, 5.082 g of dithiobenzoic acid, 8.18 g of trimethyl borate, and 5 g of silicon nitride, add 15 ml of a 75% by volume methanol aqueous solution, and stir for 1.5 h to mix thoroughly;
[0094] (2) placing the mixture at 90° C. and leaving it to stand for 0.5 h to turn it into a gel-like substance;
[0095] (3) subjecting the gel-like substance to microwave heating and drying treatment at 140° C. and 9000 Pa for 17 h;
[0096] (4) subjecting the dried mixture to high temperature treatment at 1800° C. for 2 h using a Joule heater in a helium atmosphere;
[0097] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it with butanol three times;
[0098] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0099] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 200 °C, acetylene space velocity 500 h -1 , the volume ratio of hydrogen to acetylene was 1:1; the reaction conversion rate was 89% and the ethylene selectivity was 98%.
[0100] Example 8
[0101] (1) Weigh 4.12 g of methyl diphenylphosphine oxide, 4.332 g of diphenylthiourea, 2.68 g of p-methylphenylboric acid, and 2.8 g of silicon nitride, add 15 ml of 75% by volume ethanol aqueous solution, and stir for 1.5 h to mix thoroughly;
[0102] (2) placing the mixture at 35°C for 3 hours to turn it into a gel-like substance;
[0103] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 6000 Pa for 18 h;
[0104] (4) subjecting the dried mixture to high temperature treatment at 800° C. for 10 h using a Joule heater in a helium atmosphere;
[0105] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with propanol;
[0106] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0107] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 160°C, acetylene space velocity 600h -1 , the volume ratio of hydrogen to acetylene was 0.8:1; the reaction conversion rate was 86% and the ethylene selectivity was 99%.
[0108] Example 9
[0109] (1) Weigh 11.45 g of triphenylphosphine sulfide, 5 g of benzothiazole, 1.29 g of boron oxide, and 1.40 g of silicon nitride, add 15 ml of deionized water, and stir for 1.5 h to mix thoroughly;
[0110] (2) placing the mixture at 50° C. for 2.5 h to turn it into a gel-like substance;
[0111] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 8000 Pa for 20 h;
[0112] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater under a nitrogen atmosphere;
[0113] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it with acetone three times;
[0114] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0115] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 170°C, acetylene space velocity 2000h -1 , the volume ratio of hydrogen to acetylene was 0.8:1; the reaction conversion rate was 79% and the ethylene selectivity was 99%.
[0116] Example 10
[0117] (1) Weigh 33.98 g of methyl triphenylphosphine chloride, 113.07 g of 2-aminobenzothiazole, 3.03 g of boron oxide, and 5 g of silicon nitride, add 15 ml of 5% starch aqueous solution, and stir for 1.5 h to mix thoroughly;
[0118] (2) placing the mixture at 30° C. for 2.5 h to turn it into a gel-like substance;
[0119] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 10,000 Pa for 10 h;
[0120] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater in a helium atmosphere;
[0121] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with aqueous ammonia;
[0122] (6) The washed catalyst was dried at 110° C. for 12 hours and ground to a particle size of 20 mesh; the SEM image of the material prepared in Example 10 is shown in FIG. Figure 2 It can be seen that after doping with impurity elements, a rich pore structure is generated on the surface of the material.
[0123] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 300 °C, acetylene space velocity 800 h -1 , the volume ratio of hydrogen to acetylene was 1.2:1; the reaction conversion rate was 80% and the ethylene selectivity was 98%.
[0124] Comparative Example 1
[0125] (1) Weigh 33.98 g of methyl triphenylphosphonium chloride and 5 g of silicon nitride, add 15 ml of a 5% starch aqueous solution, and stir for 1.5 h to mix thoroughly;
[0126] (2) placing the mixture at 30° C. for 2.5 h to turn it into a gel-like substance;
[0127] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 10,000 Pa for 10 h;
[0128] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater under a nitrogen atmosphere;
[0129] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with aqueous ammonia;
[0130] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0131] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 300 °C, acetylene space velocity 800 h -1 , the volume ratio of hydrogen to acetylene was 1.2:1; the reaction conversion rate was 24%, and the ethylene selectivity was 69%.
[0132] Comparative Example 2
[0133] (1) Weigh 3.03 g of boron oxide, 5 g of silicon nitride, and 5 ml of 15% starch aqueous solution, and stir for 1.5 h to mix them thoroughly;
[0134] (2) placing the mixture at 30° C. for 2.5 h to turn it into a gel-like substance;
[0135] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 10,000 Pa for 10 h;
[0136] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater in a helium atmosphere;
[0137] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with aqueous ammonia;
[0138] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0139] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 300 °C, acetylene space velocity 800 h -1 , the volume ratio of hydrogen to acetylene was 1.2:1; the reaction conversion rate was 28%, and the ethylene selectivity was 30%.
[0140] Comparative Example 3
[0141] (1) Weigh 5.082 g of dithiobenzoic acid and 5 g of silicon nitride, add 15 ml of 5% starch aqueous solution, and stir for 1.5 h to mix thoroughly;
[0142] (2) placing the mixture at 30° C. for 2.5 h to turn it into a gel-like substance;
[0143] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 10,000 Pa for 10 h;
[0144] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater in a helium atmosphere;
[0145] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with aqueous ammonia;
[0146] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0147] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 300 °C, acetylene space velocity 800 h -1 , the volume ratio of hydrogen to acetylene was 1.2:1; the reaction conversion rate was 26%, and the ethylene selectivity was 84%.
[0148] Comparative Example 4
[0149] (1) Weigh 33.98 g of methyl triphenylphosphine chloride, 3.03 g of boron oxide, and 5 g of silicon nitride, add 15 ml of 5% starch aqueous solution, and stir for 1.5 h to mix thoroughly;
[0150] (2) placing the mixture at 30° C. for 2.5 h to turn it into a gel-like substance;
[0151] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 10,000 Pa for 10 h;
[0152] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater in a helium atmosphere;
[0153] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with aqueous ammonia;
[0154] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0155] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 300 °C, acetylene space velocity 800 h -1 , the volume ratio of hydrogen to acetylene was 1.2:1; the reaction conversion rate was 47% and the ethylene selectivity was 90%.
[0156] Comparative Example 5
[0157] (1) Weigh 33.98 g of methyl triphenylphosphonium chloride, 113.07 g of 2-aminobenzothiazole, and 5 g of silicon nitride, add 15 ml of 5% starch aqueous solution, and stir for 1.5 h to mix thoroughly;
[0158] (2) placing the mixture at 30° C. for 2.5 h to turn it into a gel-like substance;
[0159] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 10,000 Pa for 10 h;
[0160] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater in a helium atmosphere;
[0161] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with aqueous ammonia;
[0162] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0163] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 300 °C, acetylene space velocity 800 h -1 , the volume ratio of hydrogen to acetylene was 1.2:1; the reaction conversion rate was 53% and the ethylene selectivity was 92%.
[0164] Comparative Example 6
[0165] (1) Weigh 113.07 g of 2-aminobenzothiazole, 3.03 g of boron oxide, and 5 g of silicon nitride, add 15 ml of 5% starch aqueous solution, and stir for 1.5 h to mix thoroughly;
[0166] (2) placing the mixture at 30° C. for 2.5 h to turn it into a gel-like substance;
[0167] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 10,000 Pa for 10 h;
[0168] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater in a helium atmosphere;
[0169] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with aqueous ammonia;
[0170] (6) drying the washed catalyst at 110° C. for 12 hours and grinding the catalyst to a particle size of 20 mesh;
[0171] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 300 °C, acetylene space velocity 800 h -1 , the volume ratio of hydrogen to acetylene was 1.2:1; the reaction conversion rate was 57% and the ethylene selectivity was 94%.
[0172] Comparative Example 7
[0173] (1) Weigh 5 g of original silicon nitride, add 15 ml of aqueous solution, and stir for 1.5 h to mix thoroughly;
[0174] (2) placing the mixture at 30° C. and leaving it to stand for 2.5 hours to obtain a gel-like substance;
[0175] (3) subjecting the gel-like substance to microwave heating and drying at 140° C. and 10,000 Pa for 10 h;
[0176] (4) subjecting the dried mixture to high temperature treatment at 1600° C. for 6 h using a Joule heater in a helium atmosphere;
[0177] (5) cooling the catalyst after the high temperature treatment to room temperature and washing it three times with aqueous ammonia;
[0178] (6) The washed catalyst was dried at 110°C for 12 hours and ground to a particle size of 20 mesh; the SEM image of the material obtained in Comparative Example 7 is shown in Figure 1 It can be seen that before doping with impurity elements, the surface of the material is relatively smooth and there are a small number of pores.
[0179] (7) Evaluation of acetylene hydrogenation reaction in a fixed bed reactor: Acetylene hydrogenation reaction at 300 °C, acetylene space velocity 800 h -1 , the volume ratio of hydrogen to acetylene was 1.2:1; the reaction conversion rate was 13%, and the ethylene selectivity was 82%.
[0180] The porous property parameters of the porous silicon nitride materials prepared in some embodiments and comparative examples of the present invention are shown in Table 1. As can be seen from the data in Table 1, the preparation method of the silicon nitride material adopted in the present invention greatly increases the specific surface area and pore volume of the material, and gives the silicon nitride porous properties.
[0181] Table 1: Porous property parameters of porous silicon nitride materials
[0182]
Claims
1. A method for preparing a porous silicon nitride material doped with hetero-elements, characterized in that: The preparation method comprises the following steps: 1) Fully mixing a phosphorus-containing precursor, a sulfur-containing precursor, a boron-containing precursor, silicon nitride and a solvent, and stirring to obtain a mixture; the feeding ratio of the phosphorus-containing precursor, the sulfur-containing precursor, the boron-containing precursor and the silicon nitride is according to the element molar ratio of phosphorus: sulfur: boron: nitrogen = 0.1~1: 0.1~1: 0.5~5; 2) allowing the mixture obtained in step 1) to stand to obtain a gel-like substance; 3) subjecting the gel-like substance obtained in step 2) to microwave heating and drying treatment, wherein the drying temperature is 60-150° C., the vacuum degree is 100-100000 Pa, and the drying time is 2-20 h; 4) subjecting the mixture after the drying treatment in step 3) to high temperature treatment using a Joule heating apparatus, wherein the temperature of the high temperature treatment is 300-1800° C.; the time of the high temperature treatment is 1-30 hours; and the atmosphere of the high temperature treatment is an inert atmosphere; 5) Cooling the mixture after high temperature treatment in step 4) to room temperature, washing, drying and grinding to obtain a heteroelement-doped porous silicon nitride material, wherein the molar ratio of nitrogen to silicon in the silicon nitride material is 4:
3.
2. The preparation method according to claim 1, characterized in that: The phosphorus-containing precursor in step 1) is selected from one or more of hydroxyethylidene diphosphonic acid, (2-hydroxyethyl) benzenephosphonic acid, tetraphenylphosphine chloride, ethyl dichlorophosphate, pyrophosphoric acid, methyl diphenylphosphine oxide, metaphosphoric acid, triphenylphosphine sulfide and methyl triphenylphosphine chloride.
3. The preparation method according to claim 1, characterized in that: The sulfur-containing precursor in step 1) is selected from one or more of diphenyl sulfoxide, diphenylthiourea, dithiobenzoic acid, 2-thiophenecarboxylic acid, sodium diethyldithiocarbamate, diphenyl disulfide, benzothiazole and 2-aminobenzothiazole.
4. The preparation method according to claim 1, characterized in that: The boron-containing precursor in step 1) is selected from one or more of boric acid, trimethyl borate, triethyl borate, phenylboric acid, p-hydroxyphenylboric acid, p-methylphenylboric acid and boron oxide.
5. The preparation method according to claim 1, characterized in that: The solvent in step 1) is selected from at least one of water, methanol, ethanol, acetone, sucrose aqueous solution and starch aqueous solution.
6. The preparation method according to claim 1, characterized in that: In step 2), the mixture is placed at a temperature between room temperature and 90° C. for a time between 0.5 and 3 hours.
7. A heteroelement-doped porous silicon nitride material prepared according to the preparation method according to any one of claims 1 to 6.
8. Use of the heteroelement-doped porous silicon nitride material as claimed in claim 7 as a catalyst in the selective hydrogenation reaction of acetylene.
Citation Information
Patent Citations
High-dispersion transition metal catalyst anchored to silicon nitride and preparation method and application thereof
CN114433246A
Cu / silicon nitride catalyst and preparation method and application thereof
CN116273136A
Method and catalyst for direct oxygen-free preparation of olefins from methane
CN104148101A
Environment-friendly acetylene hydrochlorination catalyst and preparation method thereof
CN110743616A