A sensor based on Fe3O4 / CuCo2S4 and its application in detecting microplastic co-pollutants

The Fe3O4/CuCo2S4-based sensor addresses the limitations of existing detection methods by providing a portable and sensitive PEC POCT system for microplastic co-pollutants, achieving broad detection ranges and low limits of detection for DBP and BaP.

CN118458837BActive Publication Date: 2024-12-03WUHAN TEXTILE UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410366981.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2024-12-03
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

Current methods for detecting microplastic co-pollutants like DBP and BaP are limited by low sensitivity, difficulty in synchronous detection, and the lack of portable, rapid on-site detection capabilities, necessitating expensive laboratory equipment and complex procedures.

Method used

A Fe3O4/CuCo2S4-based sensor is developed, utilizing a hydrothermal method to synthesize a Z-type heterojunction nanocomposite material, which is integrated into a PEC POCT sensor for simultaneous detection of DBP and BaP, employing a smartphone and portable electrochemical workstation for intelligent detection.

Benefits of technology

The sensor achieves wide detection ranges and low detection limits for DBP and BaP, with linear ranges of 1.0 pg/mL-500 ng/mL and 0.5 pg/mL-50 ng/mL, and LOD values of 0.126 pg/mL and 0.132 pg/mL, respectively, demonstrating improved sensitivity and portability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118458837B_ABST
    Figure CN118458837B_ABST
Patent Text Reader

Abstract

The present invention discloses a sensor based on Fe3O4 / CuCo2S4 and an application for detecting microplastic co-pollutants. The preparation method of the composite material comprises the following steps: S11, dispersing Fe3O4, Co(NO3)2·6H2O and Cu(NO3)2·3H2O in ultrapure water; S12, dispersing thiourea and ethylenediamine in a precursor solution and stirring them fully; S13, after the solution prepared in step S12 is reacted at 180-220°C, it is cooled to room temperature, and the product is washed alternately with ethanol and ultrapure water, and then dried in a vacuum drying oven at 50-70°C, to finally obtain the product Fe3O4 / CuCo2S4 composite material. The present invention synthesizes a Z-type heterojunction nanocomposite material, i.e., a Fe3O4 / CuCo2S4 composite material, by a hydrothermal method, and constructs a PEC POCT sensor based on the Z-type heterojunction nanocomposite material. CuCo2S4(E g :1.5-2.5eV) is a photoelectrically active material that can be used for PEC analysis. Its effective visible light adsorption and high charge separation efficiency help electrons quickly transfer to the catalyst surface and participate in the photocatalytic process. The present invention forms a composite material with Fe3O4 that has a matching potential with CuCo2S4, thereby promoting the migration of photogenerated carriers, reducing hole accumulation, and improving the detection sensitivity, reproducibility and stability of PEC POCT sensors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a sensor based on Fe3O4 / CuCo2S4 and its application in detecting microplastic co-pollutants. Background Art

[0002] As emerging pollutants, micro / nano plastics pose a serious threat to environmental and food safety issues, which are closely related to human health. Therefore, micro / nano plastics have received increasing attention. Survey results show that by 2040, global plastic production will reach 380 million tons, and the microplastics produced will reach 10 million tons. Long-term exposure to microplastics will seriously disrupt the endocrine system of humans and animals. In addition, harmful chemicals in or on microplastics have potential carcinogenicity, teratogenicity and mutagenicity during the transfer from the environment to the food chain. Dibutyl phthalate (DBP) is one of the most widely used plasticizers in my country. It is mainly used in polyvinyl chloride processing and is widely used in automobiles, pesticides, cosmetics, dyes and infant products. The van der Waals force (or hydrogen bond) between DBP and microplastics is weak, and it is easily released from microplastics. In addition, DBP is not easy to degrade (half-life is about 5-20 years), and can spread to every corner of the world through water, atmosphere and other circulation processes, causing persistent harm to the environment. DBP can also affect the production and action of male hormones in the body, interfere with the normal function of male hormones, and have reproductive and developmental toxicity. Benzo(a)pyrene (BaP) is mainly produced by incomplete combustion of organic matter. It has reproductive toxicity, genetic toxicity and immunotoxicity. It is a representative of strong carcinogens and poses a huge threat to human health. As a lipophilic organic pollutant, BaP is easily adsorbed by microplastics in water. DBP and BaP are major pollutants in the environment and food, and there is a possibility of simultaneous exposure, which in turn endangers human health. Studies have shown that DBP and BaP were observed to exist simultaneously in canned fish in the Three Gorges and Yangtze River Basin in China and Turkey. Simultaneous exposure to DBP and BaP can cause serious effects on the liver, kidneys and reproductive system. China has established strict regulations on the content of DBP and BaP: the content of DBP in edible oil is 300ng / mL, the content in drinking water is 3ng / mL, and the content of BaP in both edible oil and drinking water is 10ng / mL.

[0003] Currently, high performance liquid chromatography (HPLC), gas chromatography-mass spectrometry (GC-MS) and enzyme-linked immunosorbent assay (ELISA) have been widely used for the detection of DBP and BaP in the environment and food. These detection methods are reliable, but they rely on expensive and large laboratory instruments, have complex processing procedures and long detection times. Therefore, the above laboratory-based methods face the following challenges: (1) low sensitivity in complex matrices; (2) difficulty in synchronous detection; (3) difficulty in rapid on-site detection and difficulty in becoming a detection tool independent of the laboratory. Photoelectrochemical (PEC) point-of-care testing (POCT) is a promising alternative method with the advantages of high sensitivity, high detection flux and good portability. First, the Z-type photocathode nanomaterials in PEC POCT have excellent anti-interference and redox capabilities, which can improve the detection sensitivity. Under light irradiation, the photogenerated holes of the photocathode nanomaterials are directed to the electrode surface and captured by the electrons from the counter electrode. Therefore, the reducing substances adsorbed on the surface of the cathode material will not react with the holes of the photocathode, thereby obtaining a real photocurrent. Secondly, the multi-channel portable electrochemical workstation can achieve simultaneous detection of various targets through simple operation. Third, the application software can quickly capture and convert signals through Bluetooth to achieve on-site intelligent detection. With the above advantages, PEC POCT has now been applied in the fields of food safety and environmental monitoring. Therefore, in the process of food safety and environmental monitoring, the selection of functional photoelectric active electrodes is crucial.

[0004] Therefore, a Fe3O4 / CuCo2S4-based sensor and its application in detecting microplastic co-pollutants need to be proposed urgently. Summary of the invention

[0005] In order to solve the defects of the prior art, the present invention provides a sensor based on Fe3O4 / CuCo2S4 and its application in detecting microplastic co-pollutants.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] The first object of the present invention is to provide a method for preparing CuCo2S4, comprising the following steps:

[0008] S1. Add Co(NO3)2·6H2O and Cu(NO3)2·3H2O into a beaker, then add ultrapure water and stir to obtain a clear precursor solution;

[0009] S2, then adding thiourea and ethylenediamine to the precursor solution and stirring;

[0010] S3. Transfer the mixed solution in step S2 into a polytetrafluoroethylene reactor. After the reaction is completed at 180-220°C, cool to room temperature, wash the product alternately with ethanol and ultrapure water, and then dry it in a vacuum drying oven at 50-70°C to finally obtain the product CuCo2S4.

[0011] Preferably, in step S1, the mass ratio of Co(NO3)2·6H2O, Cu(NO3)2·3H2O and ultrapure water is 1:1:52-6:1:125, and the stirring time in step S1 is 10-20 minutes;

[0012] The mass ratio of thiourea to ethylenediamine in step S2 is in the range of 1:60-1:300, and the stirring time in step S2 is 35-45 minutes;

[0013] The reaction time in step S3 is 5-15 hours, and the drying time is 6-8 hours.

[0014] The second object of the present invention is to provide a method for preparing a Fe3O4 / CuCo2S4 composite material, comprising the following steps:

[0015] S11, disperse Fe3O4, Co(NO3)2·6H2O and Cu(NO3)2·3H2O in ultrapure water;

[0016] S12, dispersing thiourea and ethylenediamine into the precursor solution and stirring thoroughly;

[0017] S13. After the solution prepared in step S12 is reacted at 180-220°C, it is cooled to room temperature and the product is washed alternately with ethanol and ultrapure water, and then dried in a vacuum drying oven at 50-70°C to obtain a Fe3O4 / CuCo2S4 composite material.

[0018] Preferably, in step S11, the mass ratio of Fe3O4, Co(NO3)2·6H2O, Cu(NO3)2·3H2O and ultrapure water is 1:3.5:3.5:128-1:21:3.5:438; the mass ratio of Co(NO3)2·6H2O and Cu(NO3)2·3H2O in step S11 is in the range of 1:4:2-3:6:4, and the stirring time in step S1 is 10-20 minutes;

[0019] The mass ratio of thiourea to ethylenediamine in step S12 is in the range of 1:60-1:300, and the stirring time in step S2 is 35-45 minutes;

[0020] In step S13, the heating time is 8-12 hours, and the drying time is 6-8 hours.

[0021] The third object of the present invention is to provide a PEC POCT sensor based on a Fe3O4 / CuCo2S4 composite material, wherein the preparation method of the PEC POCT sensor comprises the following steps:

[0022] S21, preparing 0.5% chitosan solution: dissolving chitosan (CS) in 1% acetic acid, and sonicating;

[0023] S22, dispersing the Fe3O4 / CuCo2S4 composite material in a mixed solution of ethanol and 0.5% chitosan, drop-coating it on the surface of the ITO electrode after ultrasonic treatment, and naturally drying to obtain a Fe3O4 / CuCo2S4 / CS / ITO electrode;

[0024] S23, incubating the Fe3O4 / CuCo2S4 / CS / ITO electrode obtained in step S22 with a 2.5% glutaraldehyde (GLD) solution at room temperature, and then washing with a 0.1M PBS solution to form a GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode;

[0025] S24, drop-coating the antigen (Ag) on ​​the surface of the GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode obtained in step S23, and incubating at 4° C. to obtain an Ag / GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode;

[0026] S25. Use BSA solution to seal the excess active sites on the surface of the Ag / GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode obtained in step S24. After incubation at 37°C, rinse the electrode thoroughly with PBS to complete the construction of the BSA / Ag / GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode.

[0027] Preferably, in step S21, 0.2-0.4 g of chitosan and 1% acetic acid are added, and the ultrasonic time in step S21 is 10-20 minutes.

[0028] Preferably, in step S22, 2-5 mg of Fe3O4 / CuCo2S4 composite material is added to a mixed solution of ethanol and 0.5% chitosan, and the volume ratio of ethanol to 0.5% chitosan is 1:2-3:4; and the ultrasonic time in step S22 is 10-20 minutes.

[0029] Preferably, in step 23, 4-6 μL of 2.5% GLD solution is used, and in step S24, 0.5-10 ng of antigen is used.

[0030] Preferably, the incubation time in step S24 is 12-18 hours; and the incubation time in step S25 is 0.5-1 hour.

[0031] The fourth purpose of the present invention is to provide an application of a PEC POCT sensor based on Fe3O4 / CuCo2S4 composite material in detecting microplastic co-pollutants, wherein the PEC POCT sensor is used to detect the DBP and BaP content in the environment and food.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] The present invention synthesizes a Z-type heterojunction nanocomposite material, namely a Fe3O4 / CuCo2S4 composite material, by a hydrothermal method, and constructs a PEC POCT sensor based on the composite material. g : 1.5-2.5eV) is a photoelectrically active material that can be used for PEC analysis. Its effective visible light adsorption and high charge separation efficiency help electrons to quickly transfer to the catalyst surface and participate in the photocatalytic process, and can be used for photoelectric sensing detection. The present invention forms a composite material with Fe3O4 that has a matching potential with CuCo2S4, thereby promoting the migration of photogenerated carriers, reducing hole accumulation, and improving the activity and stability of PEC POCT sensors.

[0034] The present invention exhibits a wide detection range and a low detection limit in complex actual samples such as the environment and food. The wide linear ranges of DBP and BaP are 1.0pg / mL-500ng / mL and 0.5pg / mL-50ng / mL, respectively, and the low LOD values ​​are 0.126pg / mL and 0.132pg / mL, respectively. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 a is a schematic diagram of a PEC POCT sensor based on Fe3O4 / CuCo2S4 composite material constructed by the present invention;

[0036] Figure 1 b is a schematic diagram of the detection process of the PEC POCT sensor based on Fe3O4 / CuCo2S4 composite material of the present invention;

[0037] Figure 2 It is the XRD diagram of Fe3O4, CuCo2S4, and Fe3O4 / CuCo2S4-105 of the present invention;

[0038] Figure 3 a is a 100nm SEM image of Fe3O4 of the present invention;

[0039] Figure 3 b is a 100nm SEM image of CuCo2S4 of the present invention;

[0040] Figure 3c is a 100nm SEM image of Fe3O4 / CuCo2S4 of the present invention;

[0041] Figure 4 It is a charge transfer mechanism diagram of Fe3O4 / CuCo2S4 of the present invention;

[0042] Figure 5 a is a DBP calibration curve diagram of the present invention;

[0043] Figure 5 b is a BaP calibration curve diagram of the present invention. DETAILED DESCRIPTION

[0044] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0045] Example 1: Preparation of Fe3O4 / CuCo2S4 composite material.

[0046] First, the CuCo2S4 material was synthesized by a hydrothermal method. 0.58g Co(NO3)2·6H2O and 0.24g Cu(NO3)2·3H2O were accurately weighed and added to a 100mL beaker, and then 30mL ultrapure water was added and stirred for 10 minutes to obtain a clear precursor solution. Then 0.03g thiourea and 2mL ethylenediamine were added to the precursor solution and stirred for 35 minutes. The mixed solution was transferred to a 100mL polytetrafluoroethylene reactor and reacted at 200°C for 10 hours. After cooling to room temperature, the product was washed alternately with ethanol and ultrapure water, and then dried in a vacuum drying oven at 60°C for 8 hours to obtain the product CuCo2S4.

[0047] The Fe3O4 / CuCo2S4 composite material was synthesized using the same hydrothermal method. 0.16g Fe3O4, 0.58g Co(NO3)2·6H2O and 0.24g Cu(NO3)2·3H2O were weighed and dispersed in 30mL ultrapure water. Subsequently, 0.03g thiourea and 2mL ethylenediamine were dispersed in the precursor solution and stirred for 35 minutes. The prepared solution was heated at 200°C for 10 hours, then washed alternately with ethanol and ultrapure water, and finally dried in vacuum at 60°C to obtain the Fe3O4 / CuCo2S4 composite.

[0048] Example 2: Characterization of Fe3O4 / CuCo2S4 materials.

[0049] The phase composition and crystal structure of Fe3O4, CuCo2S4 and Fe3O4 / CuCo2S4 were characterized by XRD. Figure 2As shown, CuCo2S4 has diffraction peaks at 16.13°, 26.58°, 31.27°, 37.96°, 46.99°, 49.99° and 54.79°, which correspond to the (111), (022), (113), (004), (224), (115) and (044) crystal planes of CuCo2S4 (JCPDS No. 42-1450). The diffraction peaks at 35.42°, 43.05°, 53.39°, 56.94° and 62.52° correspond to the (311), (400), (422), (511) and (440) crystal planes of Fe3O4 (JCPDS No. 19-0629). There are obvious diffraction peaks of CuCo2S4 and Fe3O4 in Fe3O4 / CuCo2S4, which proves that the synthesis of Fe3O4 / CuCo2S4 is successful.

[0050] The carrier transfer behavior and efficiency of CuCo2S4 and Fe3O4 / CuCo2S4 were explored by PEC photocurrent-time experiments. Among CuCo2S4, the photoelectrode based on CuCo2S4 has the largest photocurrent signal. Then the photocurrent signal of the CuCo2S4 electrode was compared with that of the Fe3O4 / CuCo2S4 electrode, and it was found that the photocurrent signal of the photoelectrode based on Fe3O4 / CuCo2S4 was 1.3 times higher than that of CuCo2S4-10. The results show that Fe3O4 / CuCo2S4 has better PEC performance.

[0051] The morphologies of Fe3O4, CuCo2S4 and Fe3O4 / CuCo2S4 were observed by SEM. Fe3O4 is a uniformly distributed nanoparticle ( Figure 3 a). CuCo2S4 is a nanoflower composed of many uniformly interlaced nanosheets ( Figure 3 b). Fe3O4 / CuCo2S4 also shows a flower-like microsphere structure ( Figure 3 c), but it is obvious that nanoparticles similar to Fe3O4 are attached to the surface of Fe3O4 / CuCo2S4 nanosheets. XRD results prove the successful synthesis of Fe3O4 / CuCo2S4 materials.

[0052] Figure 4 As shown in the figure, under the action of visible light, electron-hole pairs are generated, and the electrons of Fe3O4 and CuCo2S4 migrate from CB to VB. The electrons on the CB of CuCo2S4 and the holes on the VB of Fe3O4 combine through electrostatic interaction to avoid the recombination of photogenerated carriers on Fe3O4 and CuCo2S4. In the reaction solution, the strong reducing electrons reduce the O2 in the solution to ·O 2-Therefore, we conclude that there is a Z-type heterojunction between Fe3O4 and CuCo2S4, which improves the spatial separation of carriers and redox activity.

[0053] Example 3: DFT calculations.

[0054] Based on density functional theory, DFT calculations of CuCo2S4 and Fe3O4 were performed using the Vienna Ab-initio simulation software package. The geometric structures, density of states (DOS) and work functions of CuCo2S4 and Fe3O4 were obtained by first-principles calculations. The Perdew-Burke-Ernzerhof method with generalized gradient approximation was used to describe the exchange-correlation potential. The Brillouin zone integration was performed using a plane wave cutoff energy of 500 eV and a 5×5×5 K-point grid, and the structural and electronic properties of CuCo2S4(001) and Fe3O4(001) were calculated. For the CuCo2S4(001) / Fe3O4(001) heterostructure, the plane wave cutoff energy was also set to 520 eV. Until the energy and force converge to 10 -5 eV and , all geometries are fully relaxed.

[0055] Example 4: Construction and optimization of PEC POCT sensor.

[0056] Before use, the ITO electrode was cleaned by ultrasonic cleaning with ultrapure water, anhydrous ethanol, and ultrapure water for 10 minutes in turn, and finally dried naturally.

[0057] The preparation process of Fe3O4 / CuCo2S4-based PEC POCT sensor is as follows Figure 1 a. First, prepare a 0.5% chitosan solution: dissolve 0.25g chitosan in 1% acetic acid and ultrasonicate for 10 minutes. Weigh 3mg Fe3O4 / CuCo2S4 and disperse it in a mixed solution of 200μL ethanol and 300μL 0.5% chitosan. Ultrasonicate for 10 minutes, then transfer 20μL of the mixed solution and drop it on the surface of the ITO electrode. After natural drying, an effective modified area of ​​0.5cm 2Fe3O4 / CuCo2S4 / CS / ITO electrode. Subsequently, the obtained Fe3O4 / CuCo2S4 / CS / ITO electrode was incubated with 5μL of 2.5% GLD solution (w / v) at room temperature for 0.5 hours, and then washed with 0.1M PBS solution to form a GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode. 10μL Ag (200ng / mL) was drop-coated on the surface of the above electrode and incubated at 4°C for 12 hours to obtain an Ag / GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode. Then, 10μL BSA solution (1% w / v) was used to block the excess active sites on the electrode surface, and the electrode was thoroughly rinsed with PBS after incubation at 37°C for 0.5 hours. After the BSA / Ag / GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode was constructed, it was stored in a 4°C refrigerator for use.

[0058] Intelligent detection process Figure 1 As shown in Figure b. The Fe3O4 / CuCo2S4-based PEC POCT sensor, a smartphone (Android), an application (PSTrace 5.8), and a portable high-throughput electrochemical workstation (PalmSens4) were combined to build a PEC intelligent detection platform. The PalmSens4 device was connected to two working electrodes at the same time to complete the simultaneous detection of DBP and BaP. We connected the Fe3O4 / CuCo2S4-based PEC biosensor to the portable PalmSens4 device and downloaded the PSTrace 5.8 application on the smartphone. Then, Bluetooth was introduced to connect the PalmSens4 device and the smartphone to transmit and record the test results on the smartphone.

[0059] According to the detection steps of the PEC POCT sensor mentioned above, we used the control variable method to optimize different antigen concentrations and antibody concentrations.

[0060] Example 5: PEC experiment.

[0061] All PEC experiments used a three-electrode system (ITO, SCE, and Pt electrodes) and a 300W xenon lamp (λ>420nm, Perfect Light Source, Beijing, China) as the light source. Photocurrent experiments were tested by repeatedly turning the light on (30 seconds) and off (30 seconds) in 0.1M PBS (pH=7.4). 3- / 4-Electrochemical impedance spectroscopy (EIS) experiments were performed in 20 mL KCl. The entire experiment was carried out at room temperature. The photocurrent-time curve and EIS were displayed on a smartphone via a portable PalmSens4 and PSTrace 5.8. The photocurrent change value (ΔI) was positively correlated with the measured DBP and BaP concentrations by competitive immunoassay.

[0062] Example 6: Evaluation and validation of PEC POCT sensor.

[0063] The LOD, linear range, recovery, stability, selectivity, repeatability and reproducibility of DBP and BaP were evaluated by testing the Fe3O4 / CuCo2S4-based PEC POCT sensor. First, the standard curve equation was Y=aX+b, where X was the logarithm of the concentration of DBP or BaP, and Y was the photocurrent change value (ΔI). The LOD value was calculated by the formula: LOD=AC+3SD (AC: average concentration value of blank samples, SD: standard deviation value of blank samples). The time-based photocurrent stability, long-term stability, repeatability and reproducibility were evaluated by adding DBP (50ng / mL) or BaP (0.2ng / mL) to the blank samples. Using an Fe3O4 / CuCo2S4-based electrode, the prepared PEC POCT was tested for time-based photocurrent stability in ten consecutive on / off light cycle experiments. The electrodes prepared in the same batch were stored in a 4℃ refrigerator for 5 days and then tested for photocurrent to verify the long-term stability of the PEC POCT sensor. The reproducibility of the PECPOCT sensor was tested by six parallel PEC POCTs (n=6). 400 ng / mL of typical interfering substances were added for specificity testing of DBP, such as DNOP, DMP, BBP, DINP, DEHP, AFB1, BaP, SMZ and OCT. 10 ng / mL of typical interfering substances were added for specificity testing of BaP, such as BbA, BkF, PYR, ANT, PHE, AFB1, DBP, SMZ and OCT. The sensor can be tested under conditions of temperature of 5-40°C and humidity of 20-80%. The PEC POCT was validated by a spike recovery experiment. Target substances (DBP: 2 and 400 ng / mL, BaP: 0.1 and 8 ng / mL) were detected in lake water, soybean oil and liquor samples. The results of PEC POCT were validated with those of GC-MS and HPLC. The parameters of GC-MS and HPLC are as follows.

[0064] Under optimal conditions, DBP and BaP were detected using Fe3O4 / CuCo2S4-based PEC POCT sensors. We recorded a linear relationship between target concentration and photocurrent (ΔI = I0-I). As the target concentration increased, the photocurrent increased ( Figure 5 a and Figure 5 b) The linear range of DBP is 0.001-500 ng / mL, and the linear equation of DBP is ΔI=-0.037 lgC (DBP) -0.218, R 2 =0.998. The LOD value of DBP is 12.6fg / mL (S / N=3), and the LOD is calculated from 21 blank samples. In addition, the linear range of BaP is 0.0005-50ng / mL, and the linear equation of BaP is ΔI=-0.092lgC (BaP) -0.467, R 2 =0.999. The LOD of BaP was 13.2 fg / mL (S / N=3). The developed PEC POCT method was more than 10 times higher than the results of previous studies (Table 1).

[0065] Table 1: Comparison of DBP and BaP detection results using different methods.

[0066]

[0067] Example 7: Practical application.

[0068] (1) Sample pretreatment: Water samples were collected from Shahu Lake in Wuhan, China, and soybean oil and liquor were purchased from a local market in Wuhan. Before the pretreatment experiment, a 0.22 μm filter membrane was used to remove impurities in lake water and liquid samples. The samples were pretreated according to the national standard. For DBP, according to the national standard (GB 5009.271-2016), 0.5 g of soybean oil sample was dissolved in 100 μL of n-hexane and 2 mL of acetonitrile, and then vortexed for 1 min, ultrasonically extracted for 30 min, and centrifuged for 6 min (4000 g), and the supernatant was collected. The remaining soybean oil samples were extracted repeatedly according to the above steps, and the supernatant was collected. The two supernatants were added to 2 mL of acetonitrile and shaken to mix. The extract was blown dry with a nitrogen blower and reconstituted with 0.5 mL of methanol for use. 5 mL of lake water or liquor sample was mixed with 2 mL of n-hexane and shaken for 1 min. Then, the supernatant was blown dry and reconstituted with 5 mL of methanol for use. For BaP, refer to the national standard (GB 5009.27-2016), dissolve 1.0g soybean oil sample in 5mL n-hexane and vortex for 1 minute (2500g). Then use benzopyrene molecular imprinting column for purification. Blow dry the sample and reconstitute it with 1mL methanol for later use. For lake water and liquor samples, 100mL lake water and liquor samples were extracted with 40mL and 30mL n-hexane respectively, blow dried and reconstituted with 1mL methanol for later use.

[0069] (2) The accuracy of the PEC POCT sensor was verified using real soybean oil, lake water, and liquor samples. By adding DBP and BaP to the samples, respectively, the PEC POCT sensor had good consistency with the detection results of GC-MS (DBP) or HPLC (BaP). The recoveries were 83.50%-118.50% (DBP) and 80.00%-119.63% (BaP), respectively. Therefore, the PEC POCT sensor has accuracy and practicality and can be actually applied in environmental testing and food fields.

[0070] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A PEC POCT sensor based on Fe3O4 / CuCo2S4 composite material, characterized in that: The preparation method of the PEC POCT sensor comprises the following steps: S21, preparing 0.5% chitosan solution: dissolving chitosan in 1% acetic acid, and sonicating; S22, dispersing the Fe3O4 / CuCo2S4 composite material in a mixed solution of ethanol and 0.5% chitosan, drop-coating it on the surface of the ITO electrode after ultrasonic treatment, and naturally drying to obtain a Fe3O4 / CuCo2S4 / CS / ITO electrode; S23, incubating the Fe3O4 / CuCo2S4 / CS / ITO electrode obtained in step S22 with a 2.5% glutaraldehyde solution at room temperature, and then washing with a 0.1M PBS solution to form a GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode; S24, applying the antigen dropwise to the surface of the GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode obtained in step S23, and incubating at 4°C to obtain an Ag / GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode; S25. Use BSA solution to seal the excess active sites on the surface of the Ag / GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode obtained in step S24. After incubation at 37°C, rinse the electrode thoroughly with PBS to complete the construction of the BSA / Ag / GLD / Fe3O4 / CuCo2S4 / CS / ITO electrode.

2. The PEC POCT sensor based on Fe3O4 / CuCo2S4 composite material according to claim 1, characterized in that: The mass ratio of chitosan to 1% acetic acid in step S21 is 1:10-1:25, and the ultrasonic time in step S21 is 10-20 minutes.

3. The PEC POCT sensor based on Fe3O4 / CuCo2S4 composite material according to claim 1, characterized in that: In the step S22, 2-5 mg of the Fe3O4 / CuCo2S4 composite material is added to a mixed solution of ethanol and 0.5% chitosan, wherein the volume ratio of the ethanol to the 0.5% chitosan is 1:2-3:4; the ultrasonic time in the step S22 is 10-20 minutes; the Fe3O4 / CuCo2S4 composite material is prepared by the following steps: S11, dispersing Fe3O4, Co(NO3)2·6H2O and Cu(NO3)2·3H2O in ultrapure water; the mass ratio of Fe3O4, Co(NO3)2·6H2O, Cu(NO3)2·3H2O to ultrapure water is 1:3.5:3.5:128-1:21:3.5:438, and the stirring time is 10-20 minutes; S12, dispersing thiourea and ethylenediamine in a mass ratio ranging from 1:60 to 1:300 into the precursor solution and stirring thoroughly for 35 to 45 minutes; S13, after the solution prepared in step S12 is reacted at 180-220°C, the heating time is 8-12 hours, and after cooling to room temperature, the product is washed alternately with ethanol and ultrapure water, and then dried in a vacuum drying oven at 50-70°C for 6-8 hours to finally obtain the product Fe3O4 / CuCo2S4 composite material.

4. The PEC POCT sensor based on Fe3O4 / CuCo2S4 composite material according to claim 1, characterized in that: In the step 23, 4-6 μL of 2.5% glutaraldehyde solution is used, and in the step S24, 0.5-10 ng of antigen is used.

5. The PEC POCT sensor based on Fe3O4 / CuCo2S4 composite material according to claim 1, characterized in that: The incubation time in step S24 is 12-18 hours; the incubation time in step S25 is 0.5-1 hour.

6. An application of a PEC POCT sensor based on a Fe3O4 / CuCo2S4 composite material as claimed in any one of claims 1 to 5 in detecting microplastic co-pollutants, characterized in that: The PEC POCT sensor is used to detect the DBP and BaP content in the environment and food.

Citation Information

Patent Citations

  • Copper-cobalt-sulfur nano-enzyme material as well as preparation method and antibacterial application thereof