A kind of straw for milk and preparation method thereof

By melt blending of antibacterial agents and multiblock copolymers in the straw material, an antibacterial and toughened straw is solved, and the existing straw is easily deformed and low mechanical strength in high-temperature liquids is achieved, and the excellent straw is achieved Mechanical properties and antibacterial properties meet the needs of reuse.

CN118459957BActive Publication Date: 2024-11-15云南大联塑料制品有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410728284.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-11-15
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

Existing biodegradable straws are prone to soften or deform in high-temperature liquids, have low mechanical strength, and are difficult to meet the needs of reuse. Moreover, due to protein residues, bacterial growth is restricted to one-time use.

Method used

Antibacterial agents are prepared using dimethylaminoethyl methacrylate, isoborne methacrylate and other materials, and melt blended through multiblock copolymers, isosorbate diisocyanate and other materials to form an antibacterial and toughened pipette. , the mechanical properties and antibacterial properties are improved by combining interfacial stereocomplex crystallization and reaction capacity enhancement.

Benefits of technology

The prepared straw has excellent mechanical properties and antibacterial properties, can maintain shape under high temperature conditions, and improves the reusability and safety of the straw by improving material compatibility and interface strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of straws, and discloses a straw for milk and a preparation method thereof. The method comprises the following steps: ultrasonically dispersing dimethylaminoethyl methacrylate, isobornyl methacrylate and an initiator into tetrahydrofuran, heating to 70-75°C, reflux reaction for 12-14 hours, cooling to room temperature, adding 1,3-propane sultone, keeping the temperature for reaction for 22-24 hours, rotary evaporation, washing, drying, and obtaining an antibacterial agent; melt blending a multi-block copolymer and polybutylene succinate co-butylene terephthalate, adding poly-L-lactic acid, triblock copolymer B and an antibacterial agent, melt blending, extruding, mold forming, cooling, pulling and cutting, and obtaining a straw for milk.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of straws, in particular to a milk straw and a preparation method thereof. Background Art

[0002] At present, biodegradable straws made of materials such as polylactic acid (PLA), polybutylene adipate / terephthalate (PBAT), polybutylene succinate (PBS), and polyhydroxyalkanoates (PHA) on the market still have many shortcomings in many aspects. These materials have poor heat resistance and are easily softened or deformed in high-temperature liquids, affecting the user experience. In addition, their mechanical strength is relatively low, and they are easy to break or bend, which cannot meet the use requirements of certain occasions. There are also challenges in processing performance, such as the need for specific processing equipment and processes, which leads to increased production costs. Milk is rich in protein, and these proteins remain inside the straw and easily breed bacteria, resulting in the straw being used only as a disposable item.

[0003] Therefore, it is of great significance to invent a reusable straw with antibacterial and excellent mechanical properties. Summary of the invention

[0004] The object of the present invention is to provide a milk straw and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing a milk straw comprises the following steps:

[0007] S1: dispersing dimethylaminoethyl methacrylate, isobornyl methacrylate and an initiator in tetrahydrofuran by ultrasonication, heating to 70-75°C, reflux reaction for 12-14h, cooling to room temperature, adding 1,3-propane sultone, keeping the temperature for reaction for 22-24h, rotary evaporation, washing and drying to obtain an antibacterial agent;

[0008] S2: melt-blending the multi-block copolymer, isosorbide diisocyanate, and polybutylene succinate-co-butylene terephthalate, adding poly-L-lactic acid, triblock copolymer B, and antibacterial agent, melt-blending, extruding, molding, cooling, pulling and cutting, and obtaining a milk straw.

[0009] Furthermore, in the milk straw, the proportions of each component, by mass, are 5-15 parts of the multi-block copolymer, 20-30 parts of polybutylene succinate-co-butylene terephthalate, 70-80 parts of poly-L-lactic acid, 5-10 parts of the triblock copolymer B, and 10-20 parts of the antibacterial agent.

[0010] Furthermore, the preparation method of the isosorbide diisocyanate comprises the following steps:

[0011] Add isosorbide and succinic anhydride to a reaction vessel, heat to 120-125°C and react for 22-24 hours; move the reaction system to an ice bath, cool to 0°C, add thionyl chloride and N,N-dimethylformamide, keep warm and react for 2-2.5 hours, add sodium azide, deionized water, and toluene, keep warm and react for 1-1.5 hours, heat to 110-115°C, add toluene, keep warm and react for 1-1.5 hours to obtain isosorbide diisocyanate.

[0012] Furthermore, the molar ratio of isosorbide:succinic anhydride:thionyl chloride:N,N-dimethylformamide:sodium azide is (1.5-2):(3.45-4.6):(20.7-27.6):(0.015-0.02):(7.5-10).

[0013] Furthermore, the method for preparing the multi-block copolymer comprises the following steps:

[0014] The terminal hydroxyl polybutadiene and stannous isooctanoate are added to a reaction container, and dextrorotatory lactide is added. The mixture is heated to 130-135° C. under a nitrogen atmosphere and reacted for 15-20 minutes. The mixture is cooled to room temperature, and dichloromethane is added. The reactant is precipitated into methanol and dried under vacuum to obtain a triblock copolymer A. The triblock copolymer A is added to a reaction container, and toluene, stannous isooctanoate and isosorbide diisocyanate are added under a nitrogen atmosphere. The mixture is heated to 75-80° C. and reacted for 7-8 hours. The mixture is rotary evaporated, and dichloromethane is added. The reactant is precipitated into methanol and dried under vacuum to obtain a multi-block copolymer.

[0015] Furthermore, in the triblock copolymer A, the mass ratio of terminal hydroxyl polybutadiene:dextrorotatory lactide is 1:(20-50); in the multiblock copolymer, the mass ratio of triblock copolymer A:isosorbide diisocyanate is 100:(1-2).

[0016] Furthermore, the preparation method of the triblock copolymer B comprises the following steps:

[0017] Add lithium chloride to a reaction vessel, perform vacuum combustion, purge with nitrogen, add tetrahydrofuran, 1,1-stilbene, sec-butyl lithium, and an initiator, cool the reaction system to -79--78°C, add methyl methacrylate, tert-butyl acrylate, and methyl methacrylate in sequence, react until the desired molecular weight is reached, quench, concentrate, precipitate the reactant into a methanol deionized water solution, and vacuum dry to obtain a crude copolymer; add the crude copolymer into n-butanol, add toluenesulfonic acid, heat to 130-135°C, react for 48-50 hours, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer B.

[0018] Furthermore, the structure of the triblock copolymer B is methyl methacrylate, n-butyl acrylate, and methyl methacrylate, wherein the weight average molecular weights of the block polymers are (40-50):100:(40-50) respectively; the weight average molecular weight of the triblock copolymer is 115,000-128,000; in the triblock copolymer B, the amount of toluenesulfonic acid added is 10 mol% of the molar amount of tert-butyl acrylate units in the crude copolymer.

[0019] Furthermore, the mass ratio of dimethylaminoethyl methacrylate:isobornyl methacrylate:1,3-propane sultone is 1:10:(0.5-0.6).

[0020] Furthermore, the melt blending temperature is 180-200° C. and the time is 6-8 min.

[0021] Furthermore, the initiators are all azobisisobutyronitrile.

[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0023] The present invention successfully prepares a bio-based antibacterial agent by copolymerizing dimethylaminoethyl methacrylate and isobornyl methacrylate, and then adding 1,3-propane sultone for zwitterionization. The antibacterial agent can provide zwitterions, which can enable the matrix to obtain a higher crosslinking density and improve the mechanical properties; since the synthetic raw materials dimethylaminoethyl methacrylate and isobornyl methacrylate are hydrophobic, they also have a wide range of antibacterial adhesion; the antibacterial activity against E. coli and S. aureus is attributed to the tertiary amine of polydimethylaminoethyl methacrylate in the antibacterial agent, which exists in the form of free amine (no charge) and is balanced with protonated amine (positively charged); the mechanical properties and antibacterial properties of the straw are improved.

[0024] The present invention uses polybutylene succinate co-butylene terephthalate as a toughening phase, multi-block copolymers and tri-block copolymers B as composite compatibilizers, and adopts a method combining interface stereocomposite crystallization and reactive compatibilization to toughen poly-L-lactic acid. Using a hydroxy-terminated polybutadiene soft segment as an initiator, a tri-block copolymer A is prepared by ring-opening polymerization with right-handed lactide, and then isosorbide-based diisocyanate is used as a chain extender to carry out a chain extension reaction on the tri-block copolymer A to prepare a multi-block copolymer; the multi-block copolymer is melt-blended with polybutylene succinate co-butylene terephthalate and poly-L-lactic acid in turn, and stereocomposite crystals (using the poly-D-lactic acid structure in the multi-block copolymer) are formed in situ at the interface between the poly-L-lactic acid and the polybutylene succinate co-butylene terephthalate and in the poly-L-lactic acid matrix. structure and poly (L-lactic acid structure); isosorbide-based diisocyanate is grafted as a compatibilizer into the A segment of the triblock copolymer, which solves the problem of its dispersibility in the matrix and can provide reactive compatibilization during the melt blending process. The stereocomposite crystals at the interface of the combined phases further improve the interfacial bonding strength of poly (L-lactic acid) and poly (butylene succinate co-terephthalate). The stereocomposite crystals can enhance the poly (butylene succinate co-terephthalate) solution, improve the storage modulus and complex viscosity of the blend, and greatly enhance the mechanical properties of the material. The present invention further improves the compatibility of polybutylene succinate-co-butylene terephthalate and poly(L-lactic acid) by controlling the molecular weight proportion of each block in the triblock copolymer B and the molecular weight of the triblock copolymer B. The addition of the triblock copolymer B can enhance the crystallization inhibition effect of the poly(L-lactic acid), reduce the glass transition temperature in melt blending, and thus improve the compatibility. Meanwhile, the polybutyl acrylate soft segment structure in the triblock copolymer B can further toughen the poly(L-lactic acid), and the methoxycarbonyl groups in the polymethyl methacrylate structures at both ends are similar to the ester structures in the poly(L-lactic acid) and polybutylene succinate-co-butylene terephthalate, have strong affinity, and can further improve the interface strength and mechanical properties. DETAILED DESCRIPTION

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] In the following examples, hydroxy-terminated polybutadiene CAS: 69102-90-5, Mn is 4000; poly-L-lactic acid model is 4032D, purchased from Nature Works, USA; polybutylene succinate co-butylene terephthalate model is TS159, Mw is 8.3×10 4g / mol, purchased from Shanghai Research Institute of Petrochemical Engineering, Sinopec; the rest of the raw materials were commercially available. Example 1

[0027] A method for preparing a straw for milk: S1: ultrasonically disperse 1 g of dimethylaminoethyl methacrylate, 10 g of isobornyl methacrylate, and 0.05 g of azobisisobutyronitrile in tetrahydrofuran, heat to 70°C, reflux for 12 h, cool to room temperature, add 0.5 g of 1,3-propane sultone, keep warm for 22 h, rotary evaporate, wash, and dry to obtain an antibacterial agent;

[0028] S2: 1.5 mol of isosorbide and 3.45 mol of succinic anhydride were added to a reaction vessel, heated to 120°C for reaction for 22 hours; the reaction system was moved to an ice bath, cooled to 0°C, 20.7 mol of thionyl chloride and 0.015 mol of N,N-dimethylformamide were added, and the reaction was kept warm for 2 hours, 7.5 mol of sodium azide, deionized water, and toluene were added, and the reaction was kept warm for 1 hour, and the reaction was heated to 110°C, toluene was added, and the reaction was kept warm for 1 hour to obtain isosorbide diisocyanate;

[0029] S3: 1 g of hydroxy-terminated polybutadiene and 0.06 g of stannous isooctanoate were added to a reaction container, and 20 g of right-handed lactide was added. The mixture was heated to 130°C for reaction for 15 min under a nitrogen atmosphere, cooled to room temperature, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a triblock copolymer A. 100 g of triblock copolymer A was added to a reaction container. Toluene, stannous isooctanoate, and 1 g of isosorbide diisocyanate were added under a nitrogen atmosphere. The mixture was heated to 75°C for reaction for 7 h, rotary evaporated, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a multi-block copolymer.

[0030] S4: Add lithium chloride to a reaction vessel, perform vacuum combustion, purge with nitrogen, add tetrahydrofuran, 1,1-diphenylethylene, sec-butyl lithium, and an initiator, cool the reaction system to -78°C, add methyl methacrylate, tert-butyl acrylate, and methyl methacrylate in sequence, react until the desired molecular weight is reached, quench, concentrate, precipitate the reactant into a methanol deionized water solution, and vacuum dry to obtain a crude copolymer; add the crude copolymer into n-butanol, add toluenesulfonic acid, heat to 130°C for 48 hours, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer B; wherein the weight average molecular weights of the block polymers of the triblock copolymer B are 40:100:40 respectively; the weight average molecular weight of the triblock copolymer is 115,000;

[0031] S5: 5 g of multi-block copolymer and 20 g of polybutylene succinate co-butylene terephthalate were melt-blended at 180° C. for 6 min, 80 g of poly-L-lactic acid, 5 g of triblock copolymer B and 10 g of antibacterial agent were added, melt-blended at 180° C. for 8 min, extruded, molded, cooled, and cut by traction to obtain a milk straw. Example 2

[0032] A method for preparing a straw for milk: S1: ultrasonically disperse 1 g of dimethylaminoethyl methacrylate, 10 g of isobornyl methacrylate, and 0.05 g of azobisisobutyronitrile in tetrahydrofuran, heat to 70°C, reflux for 12 h, cool to room temperature, add 0.5 g of 1,3-propane sultone, keep warm for 22 h, rotary evaporate, wash, and dry to obtain an antibacterial agent;

[0033] S2: 1.5 mol of isosorbide and 3.45 mol of succinic anhydride were added to a reaction vessel, heated to 120°C for reaction for 22 hours; the reaction system was moved to an ice bath, cooled to 0°C, 20.7 mol of thionyl chloride and 0.015 mol of N,N-dimethylformamide were added, and the reaction was kept warm for 2 hours, 7.5 mol of sodium azide, deionized water, and toluene were added, and the reaction was kept warm for 1 hour, and the reaction was heated to 110°C, toluene was added, and the reaction was kept warm for 1 hour to obtain isosorbide diisocyanate;

[0034] S3: 1 g of hydroxy-terminated polybutadiene and 0.06 g of stannous isooctanoate were added to a reaction container, and 50 g of right-handed lactide was added. The mixture was heated to 130°C for reaction for 15 min under a nitrogen atmosphere, cooled to room temperature, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a triblock copolymer A. 100 g of triblock copolymer A was added to a reaction container. Toluene, stannous isooctanoate, and 1 g of isosorbide diisocyanate were added under a nitrogen atmosphere. The mixture was heated to 75°C for reaction for 7 h, rotary evaporated, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a multi-block copolymer.

[0035] S4: Add lithium chloride to a reaction vessel, perform vacuum combustion, purge with nitrogen, add tetrahydrofuran, 1,1-diphenylethylene, sec-butyl lithium, and an initiator, cool the reaction system to -78°C, add methyl methacrylate, tert-butyl acrylate, and methyl methacrylate in sequence, react until the desired molecular weight is reached, quench, concentrate, precipitate the reactant into a methanol deionized water solution, and vacuum dry to obtain a crude copolymer; add the crude copolymer into n-butanol, add toluenesulfonic acid, heat to 130°C for 48 hours, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer B; wherein the weight average molecular weights of the block polymers of the triblock copolymer B are 40:100:40 respectively; the weight average molecular weight of the triblock copolymer is 115,000;

[0036] S5: 5 g of multi-block copolymer and 20 g of polybutylene succinate co-butylene terephthalate were melt-blended at 180° C. for 6 min, 80 g of poly-L-lactic acid, 5 g of triblock copolymer B and 10 g of antibacterial agent were added, melt-blended at 180° C. for 8 min, extruded, molded, cooled, and cut by traction to obtain a milk straw. Example 3

[0037] A method for preparing a straw for milk: S1: ultrasonically disperse 1 g of dimethylaminoethyl methacrylate, 10 g of isobornyl methacrylate, and 0.05 g of azobisisobutyronitrile in tetrahydrofuran, heat to 70°C, reflux for 12 h, cool to room temperature, add 0.5 g of 1,3-propane sultone, keep warm for 22 h, rotary evaporate, wash, and dry to obtain an antibacterial agent;

[0038] S2: 1.5 mol of isosorbide and 3.45 mol of succinic anhydride were added to a reaction vessel, heated to 120°C for reaction for 22 hours; the reaction system was moved to an ice bath, cooled to 0°C, 20.7 mol of thionyl chloride and 0.015 mol of N,N-dimethylformamide were added, and the reaction was kept warm for 2 hours, 7.5 mol of sodium azide, deionized water, and toluene were added, and the reaction was kept warm for 1 hour, and the reaction was heated to 110°C, toluene was added, and the reaction was kept warm for 1 hour to obtain isosorbide diisocyanate;

[0039] S3: 1 g of hydroxy-terminated polybutadiene and 0.06 g of stannous isooctanoate were added to a reaction container, and 50 g of right-handed lactide was added. The mixture was heated to 130°C for reaction for 15 min under a nitrogen atmosphere, cooled to room temperature, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a triblock copolymer A. 100 g of the triblock copolymer A was added to a reaction container. Toluene, stannous isooctanoate, and 2 g of isosorbide diisocyanate were added under a nitrogen atmosphere. The mixture was heated to 75°C for reaction for 7 h, rotary evaporated, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a multi-block copolymer.

[0040] S4: Add lithium chloride to a reaction vessel, perform vacuum combustion, purge with nitrogen, add tetrahydrofuran, 1,1-diphenylethylene, sec-butyl lithium, and an initiator, cool the reaction system to -78°C, add methyl methacrylate, tert-butyl acrylate, and methyl methacrylate in sequence, react until the desired molecular weight is reached, quench, concentrate, precipitate the reactant into a methanol deionized water solution, and vacuum dry to obtain a crude copolymer; add the crude copolymer into n-butanol, add toluenesulfonic acid, heat to 130°C for 48 hours, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer B; wherein the weight average molecular weights of the block polymers of the triblock copolymer B are 40:100:40 respectively; the weight average molecular weight of the triblock copolymer is 115,000;

[0041] S5: 5 g of multi-block copolymer and 20 g of polybutylene succinate co-butylene terephthalate were melt-blended at 180° C. for 6 min, 80 g of poly-L-lactic acid, 5 g of triblock copolymer B and 10 g of antibacterial agent were added, melt-blended at 180° C. for 8 min, extruded, molded, cooled, and cut by traction to obtain a milk straw. Example 4

[0042] A method for preparing a straw for milk: S1: ultrasonically disperse 1 g of dimethylaminoethyl methacrylate, 10 g of isobornyl methacrylate, and 0.05 g of azobisisobutyronitrile in tetrahydrofuran, heat to 70°C, reflux for 12 h, cool to room temperature, add 0.5 g of 1,3-propane sultone, keep warm for 22 h, rotary evaporate, wash, and dry to obtain an antibacterial agent;

[0043] S2: 1.5 mol of isosorbide and 3.45 mol of succinic anhydride were added to a reaction vessel, heated to 120°C for reaction for 22 hours; the reaction system was moved to an ice bath, cooled to 0°C, 20.7 mol of thionyl chloride and 0.015 mol of N,N-dimethylformamide were added, and the reaction was kept warm for 2 hours, 7.5 mol of sodium azide, deionized water, and toluene were added, and the reaction was kept warm for 1 hour, and the reaction was heated to 110°C, toluene was added, and the reaction was kept warm for 1 hour to obtain isosorbide diisocyanate;

[0044] S3: 1 g of hydroxy-terminated polybutadiene and 0.06 g of stannous isooctanoate were added to a reaction container, and 50 g of right-handed lactide was added. The mixture was heated to 130°C for reaction for 15 min under a nitrogen atmosphere, cooled to room temperature, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a triblock copolymer A. 100 g of the triblock copolymer A was added to a reaction container. Toluene, stannous isooctanoate, and 2 g of isosorbide diisocyanate were added under a nitrogen atmosphere. The mixture was heated to 75°C for reaction for 7 h, rotary evaporated, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a multi-block copolymer.

[0045] S4: Add lithium chloride to a reaction vessel, perform vacuum combustion, purge with nitrogen, add tetrahydrofuran, 1,1-diphenylethylene, sec-butyl lithium, and an initiator, cool the reaction system to -78°C, add methyl methacrylate, tert-butyl acrylate, and methyl methacrylate in sequence, react until the desired molecular weight is reached, quench, concentrate, precipitate the reactant into a methanol deionized water solution, and vacuum dry to obtain a crude copolymer; add the crude copolymer into n-butanol, add toluenesulfonic acid, heat to 130°C for 48 hours, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer B; wherein the weight average molecular weights of the block polymers of the triblock copolymer B are 50:100:50 respectively; the weight average molecular weight of the triblock copolymer is 128,000;

[0046] S5: 5 g of multi-block copolymer and 20 g of polybutylene succinate co-butylene terephthalate were melt-blended at 180° C. for 6 min, 80 g of poly-L-lactic acid, 5 g of triblock copolymer B and 10 g of antibacterial agent were added, melt-blended at 180° C. for 8 min, extruded, molded, cooled, and cut by traction to obtain a milk straw. Example 5

[0047] A method for preparing a straw for milk: S1: ultrasonically disperse 1 g of dimethylaminoethyl methacrylate, 10 g of isobornyl methacrylate, and 0.05 g of azobisisobutyronitrile in tetrahydrofuran, heat to 70°C, reflux for 12 h, cool to room temperature, add 0.5 g of 1,3-propane sultone, keep warm for 22 h, rotary evaporate, wash, and dry to obtain an antibacterial agent;

[0048] S2: 1.5 mol of isosorbide and 3.45 mol of succinic anhydride were added to a reaction vessel, heated to 120°C for reaction for 22 hours; the reaction system was moved to an ice bath, cooled to 0°C, 20.7 mol of thionyl chloride and 0.015 mol of N,N-dimethylformamide were added, and the reaction was kept warm for 2 hours, 7.5 mol of sodium azide, deionized water, and toluene were added, and the reaction was kept warm for 1 hour, and the reaction was heated to 110°C, toluene was added, and the reaction was kept warm for 1 hour to obtain isosorbide diisocyanate;

[0049] S3: 1 g of hydroxy-terminated polybutadiene and 0.06 g of stannous isooctanoate were added to a reaction container, and 50 g of right-handed lactide was added. The mixture was heated to 130°C for reaction for 15 min under a nitrogen atmosphere, cooled to room temperature, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a triblock copolymer A. 100 g of the triblock copolymer A was added to a reaction container. Toluene, stannous isooctanoate, and 2 g of isosorbide diisocyanate were added under a nitrogen atmosphere. The mixture was heated to 75°C for reaction for 7 h, rotary evaporated, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a multi-block copolymer.

[0050] S4: Add lithium chloride to a reaction vessel, perform vacuum combustion, purge with nitrogen, add tetrahydrofuran, 1,1-diphenylethylene, sec-butyl lithium, and an initiator, cool the reaction system to -78°C, add methyl methacrylate, tert-butyl acrylate, and methyl methacrylate in sequence, react until the desired molecular weight is reached, quench, concentrate, precipitate the reactant into a methanol deionized water solution, and vacuum dry to obtain a crude copolymer; add the crude copolymer into n-butanol, add toluenesulfonic acid, heat to 130°C for 48 hours, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer B; wherein the weight average molecular weights of the block polymers of the triblock copolymer B are 50:100:50 respectively; the weight average molecular weight of the triblock copolymer is 128,000;

[0051] S5: 15 g of multi-block copolymer and 30 g of polybutylene succinate co-butylene terephthalate were melt-blended at 180° C. for 6 min, 70 g of poly-L-lactic acid, 10 g of triblock copolymer B and 10 g of antibacterial agent were added, melt-blended at 180° C. for 8 min, extruded, molded, cooled, and cut by traction to obtain a milk straw.

[0052] Comparative Example 1: A method for preparing a straw for milk: S4: Add lithium chloride to a reaction container, vacuum burn, purge with nitrogen, add tetrahydrofuran, 1,1-diphenylethylene, sec-butyl lithium, and an initiator, cool the reaction system to -78°C, add methyl methacrylate, tert-butyl acrylate, and methyl methacrylate in sequence, react until the desired molecular weight is reached, quench, concentrate, precipitate the reactant into a methanol deionized water solution, and vacuum dry to obtain a crude copolymer; add the crude copolymer into n-butanol, add toluenesulfonic acid, heat to 130°C for 48h, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer B; wherein the weight average molecular weights of the block polymers of the triblock copolymer B are 20:100:20 respectively; the weight average molecular weight of the triblock copolymer is 115000;

[0053] The remaining steps are the same as those in Example 1.

[0054] Comparative Example 2: A method for preparing a straw for milk: S4: Add lithium chloride to a reaction container, vacuum burn, purge with nitrogen, add tetrahydrofuran, 1,1-diphenylethylene, sec-butyl lithium, and an initiator, cool the reaction system to -78°C, add methyl methacrylate, tert-butyl acrylate, and methyl methacrylate in sequence, react until the desired molecular weight is reached, quench, concentrate, precipitate the reactant into a methanol deionized water solution, and vacuum dry to obtain a crude copolymer; add the crude copolymer into n-butanol, add toluenesulfonic acid, heat to 130°C for 48h, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer B; wherein the weight average molecular weights of the block polymers of the triblock copolymer B are 50:100:50 respectively; the weight average molecular weight of the triblock copolymer is 78000;

[0055] The remaining steps are the same as those in Example 1.

[0056] Comparative Example 3: A method for preparing a straw for milk: S3: 1 g of hydroxy-terminated polybutadiene and 0.06 g of stannous isooctanoate were added to a reaction container, 20 g of L-lactide were added, and the mixture was heated to 130°C for reaction for 15 min under a nitrogen atmosphere, cooled to room temperature, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a triblock copolymer A; 100 g of the triblock copolymer A was added to a reaction container, and toluene, stannous isooctanoate, and 1 g of isosorbide diisocyanate were added under a nitrogen atmosphere, heated to 75°C for reaction for 7 h, rotary evaporated, and dichloromethane was added. The reactant was precipitated into methanol and dried under vacuum to obtain a multi-block copolymer;

[0057] The remaining steps are the same as those in Example 1.

[0058] Experiment: Mechanical properties test: According to GB / T1040-2006, a universal testing machine was used to extrude the sample into a dumbbell-shaped specimen for tensile test. The tensile rate was 20 mm / min, the test conditions were room temperature, and the average value was taken after 5 tests.

[0059] Antibacterial performance test: The antibacterial performance of the pipette was evaluated with two pathogenic bacteria, Gram-negative Escherichia coli (E.coli) and Gram-positive Staphylococcus aureus (S.aureus); the sample was squeezed out and prepared into a film, and the film samples were placed in a disposable sterile plate in groups using sterile tweezers. The prepared bacterial suspension was diluted to 10^6CFU / mL with LB liquid culture medium, and then 200μL of the diluted bacterial solution was drawn and added to the sample. The sterile plate was placed in a constant temperature incubator and incubated at 37℃ for 18 hours. After the incubation, the above common culture medium was diluted 10 times continuously with a sterilized PBS solution (three dilution ratios were used in this test: 10^5, 10^6, and 10^7). On the LB solid culture medium, 100μL of diluent was used for fermentation at a constant temperature of 37℃ for 18 hours. After the fermentation, the plate was removed, photographed, and the number of colonies was counted to calculate the antibacterial rate.

[0060] Table 1 Straw performance test data table

[0061]

[0062] Conclusion: The straw prepared by the present invention has excellent mechanical properties and antibacterial properties.

[0063] In Comparative Example 1, the molecular weight ratio of the copolymers at both ends of the triblock copolymer B was changed, resulting in decreased compatibility and reduced mechanical properties;

[0064] Comparative Example 2 reduces the weight average molecular weight of triblock copolymer B, resulting in a weakened entanglement between the segments of triblock copolymer B and poly(L-lactic acid) and poly(butylene succinate-co-butylene terephthalate) segments, an increase in the glass transition temperature of the matrix, and a decrease in the compatibility of the blend and a decrease in the mechanical properties;

[0065] In Comparative Example 3, the dextrorotatory lactide in the multi-block copolymer is replaced with l-lactide, resulting in a lack of stereocomplex crystals in the structure, leading to reduced mechanical properties.

[0066] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a milk straw, characterized in that: The following steps are involved: S1: dispersing dimethylaminoethyl methacrylate, isobornyl methacrylate and an initiator in tetrahydrofuran by ultrasonication, heating to 70-75°C, reflux reaction for 12-14h, cooling to room temperature, adding 1,3-propane sultone, keeping the temperature for reaction for 22-24h, rotary evaporation, washing and drying to obtain an antibacterial agent; S2: melt-blending the multi-block copolymer and polybutylene succinate-co-butylene terephthalate, adding poly-L-lactic acid, triblock copolymer B, and antibacterial agent, melt-blending, extruding, molding, cooling, pulling and cutting, and obtaining a milk straw; In the milk straw, the proportions of the components are, by weight, 5-15 parts of the multi-block copolymer, 20-30 parts of polybutylene succinate-co-butylene terephthalate, 70-80 parts of poly-L-lactic acid, 5-10 parts of the triblock copolymer B, and 10-20 parts of the antibacterial agent; The method for preparing the multi-block copolymer comprises the following steps: Add terminal hydroxyl polybutadiene and stannous isooctanoate to a reaction container, add dextrorotatory lactide, heat to 130-135°C under a nitrogen atmosphere, react for 15-20 minutes, cool to room temperature, add dichloromethane, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer A; add triblock copolymer A to a reaction container, add toluene, stannous isooctanoate, and isosorbide diisocyanate under a nitrogen atmosphere, heat to 75-80°C, react for 7-8 hours, rotary evaporate, add dichloromethane, precipitate the reactant into methanol, and vacuum dry to obtain a multi-block copolymer; The preparation method of the isosorbide diisocyanate comprises the following steps: Add isosorbide and succinic anhydride to a reaction vessel, heat to 120-125°C and react for 22-24 hours; move the reaction system to an ice bath, cool to 0°C, add thionyl chloride and N,N-dimethylformamide, keep warm for 2-2.5 hours, add sodium azide, deionized water, and toluene, keep warm for 1-1.5 hours, heat to 110-115°C, add toluene, keep warm for 1-1.5 hours, and obtain isosorbide diisocyanate; The preparation method of the triblock copolymer B comprises the following steps: Add lithium chloride to a reaction vessel, perform vacuum combustion, purge with nitrogen, add tetrahydrofuran, 1,1-diphenylethylene, sec-butyl lithium, and an initiator, cool the reaction system to -79--78°C, add methyl methacrylate, tert-butyl acrylate, and methyl methacrylate in sequence, react until the desired molecular weight is reached, quench, concentrate, precipitate the reactant into a methanol deionized water solution, and vacuum dry to obtain a crude copolymer; add the crude copolymer into n-butanol, add toluenesulfonic acid, heat to 130-135°C, react for 48-50 hours, precipitate the reactant into methanol, and vacuum dry to obtain a triblock copolymer B; The structure of the triblock copolymer B is methyl methacrylate, n-butyl acrylate, and methyl methacrylate, wherein the weight average molecular weights of the block polymers are (40-50):100:(40-50) respectively; the weight average molecular weight of the triblock copolymer is 115,000-128,000; in the triblock copolymer B, the amount of toluenesulfonic acid added is 10 mol% of the molar amount of tert-butyl acrylate units in the crude copolymer.

2. The method for preparing a milk straw according to claim 1, characterized in that: The molar ratio of isosorbide:succinic anhydride:thionyl chloride:N,N-dimethylformamide:sodium azide is (1.5-2):(3.45-4.6):(20.7-27.6):(0.015-0.02):(7.5-10).

3. The method for preparing a milk straw according to claim 1, characterized in that: In the triblock copolymer A, the mass ratio of terminal hydroxyl polybutadiene:dextrorotatory lactide is 1:(20-50); in the multiblock copolymer, the mass ratio of triblock copolymer A:isosorbide diisocyanate is 100:(1-2).

4. The method for preparing a milk straw according to claim 1, characterized in that: The mass ratio of dimethylaminoethyl methacrylate: isobornyl methacrylate: 1,3-propane sultone is 1:10:(0.5-0.6).

5. A straw prepared according to the method for preparing a milk straw according to any one of claims 1 to 4.