Boron-modified silicone resin high temperature resistant coating and preparation method thereof
By introducing boron elements and nanoparticles into silicone resin, combined with silane coupling agents and rigid aromatic compounds, boron-modified silicone resin coatings are prepared, which solves the problem of insufficient adhesion and mechanical strength of traditional coatings at high temperatures. It achieves better high temperature resistance and thermal stability and expands the scope of application.
Patent Information
- Application Number
- CN202410561910.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-05-08
AI Technical Summary
Traditional silicone resin coatings are prone to discoloration, cracking, and peeling at higher temperatures, and have low adhesion and mechanical strength, limiting their wide application.
Boron-containing epoxy resins are produced by combining epichlorohydrin with polymerizable boric acid and combined with tris(dimethylsiloxanyl)phenylsilane to obtain boron-containing epoxy silicone monomers, followed by silane coupling Modified with agents and nanoparticles, and finally blended with rigid aromatic compounds and silicone resin to prepare a boron-modified silicone resin high-temperature resistant coating to improve its high temperature resistance, mechanical properties and thermal stability.
It significantly improves the high-temperature resistance, mechanical properties and thermal stability of the coating, enhances the adhesion of the coating at high temperatures, avoids discoloration and peeling, improves the overall performance of the coating, and expands its application scope.
Smart Images

Figure BDA0004828025680000161
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of high temperature resistant coatings, and in particular, relates to a boron modified silicone resin high temperature resistant coating and a preparation method thereof. Background Art
[0002] Paint is a viscous liquid coated on the surface of an object to be protected or decorated, and can form a continuous film that is firmly attached to the object. It is usually mainly resin, oil or emulsion, with or without pigments, fillers, and corresponding additives, and is prepared with organic solvents or water. As a protective layer in daily production and life, paint has a very wide range of applications, so its application environment is also very wide, and it is inevitably used in environments with higher temperatures. However, due to its own physical and chemical properties, paint is often easy to soften and fall off in a high temperature environment, and thus cannot protect the product it is originally attached to, causing the product to be eroded by the external environment. Therefore, it is very important to find a paint with good high temperature resistance.
[0003] The commonly used high temperature resistant coating silicone resin coating on the market has excellent properties such as high temperature resistance, weather resistance and chemical temperature resistance. However, with the development of industrialization, people have higher and higher requirements for the comprehensive performance of high temperature resistant coatings. Traditional silicone resin coatings are prone to discoloration, cracking and falling off at high temperatures. There are disadvantages such as low adhesion and low mechanical strength of the coating at high temperatures, which limit its wide application. Based on this, the present application proposes a boron modified silicone resin high temperature resistant coating. Summary of the invention
[0004] The purpose of the present invention is to provide a boron-modified silicone resin high-temperature resistant coating and a preparation method thereof. The boron-containing epoxy resin is prepared by combining epichlorohydrin with polymerizable boric acid. The polymerizable boric acid provides carbon-carbon double bonds and hydroxyl groups for subsequent reactions, and the boron element in the polymerizable boric acid can improve the high-temperature resistance of the silicone resin. The boron-containing epoxy resin is combined with tri(dimethylsiloxane)phenylsilane to obtain a boron-containing epoxy silicone monomer. The boron-containing epoxy resin provides epoxy groups for subsequent reactions, thereby improving the heat resistance of tri(dimethylsiloxane)phenylsilane. The boron-containing epoxy silicone monomer is modified by a silane coupling agent and nanoparticles to obtain a modified silicone monomer. The cross-linking agent increases the dispersibility and hydrophobicity of the nanoparticles in the boron-containing epoxy silicone monomer, and the nanoparticles improve the mechanical properties of the boron-containing epoxy silicone monomer; the rigid aromatic compound, the modified silicone monomer and the silicone resin are blended to obtain the boron-modified silicone resin, and the rigid aromatic compound and the modified silicone monomer enhance the high temperature resistance and mechanical properties of the silicone resin; the boron-modified silicone resin, the composite inorganic pigment, the silicate filler, the curing agent, the film-forming agent, the dispersant, the thickener and the hydroxyethyl cellulose are uniformly mixed to finally obtain the boron-modified silicone resin high temperature resistant coating, which generally improves the high temperature resistance, mechanical properties and thermal stability of the coating, and improves its comprehensive performance.
[0005] The technical problem to be solved by the present invention is that the traditional organic silicone resin coating is easy to change color, crack and fall off at high temperature, and has the disadvantages of low adhesion and low mechanical strength at high temperature, which limits its wide application.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A boron-modified silicone resin high temperature resistant coating, comprising the following raw materials in parts by weight: 35-45 parts of boron-modified silicone resin, 8-12 parts of composite inorganic pigment, 5-10 parts of silicate filler, 12-15 parts of curing agent, 4-6 parts of film-forming agent, 3-5 parts of dispersant, 4-6 parts of thickener and 3-5 parts of hydroxyethyl cellulose;
[0008] The boron-modified silicone resin is prepared by blending a rigid aromatic compound, a modified silicone monomer and a silicone resin; the modified silicone monomer is prepared by modifying a boron-containing epoxy silicone monomer with a silane coupling agent and nanoparticles; the boron-containing epoxy silicone monomer is prepared by combining a boron-containing epoxy resin with tri(dimethylsiloxy)phenylsilane; the boron-containing epoxy resin is prepared by combining epichlorohydrin with polymerizable boric acid.
[0009] Further, the boron-modified organosilicon resin is prepared by the following steps:
[0010] The rigid aromatic compound is dissolved in ethanol, and then the modified silicone monomer and silicone resin are added, and stirred at 70-90°C for 6-8h. After filtering, it is washed with deionized water, and then distilled under reduced pressure at 120-140°C for 1-2h, and finally cooled to room temperature to obtain a boron-modified silicone resin, wherein the amount ratio of the rigid aromatic compound, ethanol, modified silicone monomer and modified silicone resin is 0.8-1.2g:20-30mL:0.8-1.2g:3.8-4.2g.
[0011] In the above reaction process, the rigid aromatic compound and the silicone resin have hydroxyl groups, and the surface of the nanoparticles in the modified silicone monomer has unreacted hydroxyl groups. The hydroxyl groups on the nanoparticles act as hydroxyl catalysts between the silicone resin and the rigid aromatic compound. After chemical blending, a boron-modified silicone resin with good heat resistance is obtained.
[0012] Furthermore, the rigid aromatic compound is 3-hydroxy-1,2,3-benzotriazine-4(3H)-one.
[0013] Furthermore, the organic silicone resin is methylphenyl organic silicone resin.
[0014] Furthermore, the methylphenyl silicone resin is prepared by the following steps:
[0015] 100 g of deionized water and 1 g of anion exchange resin D296R were mixed evenly, then heated to 85° C., 19.8 g of phenyltrimethoxysilane and 54.5 g of methylphenyldimethoxysilane were added, and stirring was continued at 85° C. for 2 h. The residual anion exchange resin D296R was removed by filtration, and then the residual deionized water was removed by reduced pressure distillation at -0.096 MPa and 100° C., and finally cooled to room temperature to obtain methylphenyl silicone resin.
[0016] Furthermore, the modified silicone monomer is prepared by the following steps:
[0017] The nanoparticles, silane coupling agent and ethanol solution are mixed evenly, and then stirred for 2-4 hours at 50-70°C in a nitrogen atmosphere, and then the boron-containing epoxy silicone monomer is added and the reaction is continued for 2-4 hours, and then heated to 85-95°C to remove ethanol, and finally cooled to room temperature to obtain a modified silicone monomer, wherein the amount ratio of the nanoparticles, the silane coupling agent, the ethanol solution and the boron-containing epoxy silicone monomer is 0.8-1.2g:2.8-3.2g:140-160mL:18-22g.
[0018] In the above reaction process, the nanoparticles have hydroxyl groups, and the silane coupling agent has silanol groups after hydrolysis. The hydroxyl groups on the nanoparticles can be combined with the silanol groups on the silane coupling agent to graft the silane coupling agent onto the surface of the nanoparticles. The epoxy groups on the boron-containing epoxy silicone monomer can be combined with the amino groups on the silane coupling agent to combine the nanoparticles with the boron-containing epoxy silicone monomer to finally obtain a modified silicone monomer.
[0019] Furthermore, the nanoparticles are boron nitride particles or carbon nanotubes.
[0020] Furthermore, the silane coupling agent is KH550.
[0021] Furthermore, the boron-containing epoxy silicone monomer is prepared by the following steps:
[0022] A1: Phenylsilanetriol, dimethylchlorosilane, toluene and pyridine are mixed and stirred at reflux for 6-8h. After filtering, the mixture is washed with deionized water for 3-5 times and dried with anhydrous magnesium sulfate. The solvent is then removed by rotary distillation and then vacuum distillation is performed to obtain tri(dimethylsiloxy)phenylsilane, wherein the amount ratio of phenylsilanetriol, dimethylchlorosilane, toluene and pyridine is 4.5-5.5g:15.5-16.5g:80-120mL:11-12g;
[0023] A2: Mix boron-containing epoxy resin, toluene and catalyst, and react at 65-75°C under nitrogen protection for 0.5-1.5h, then add tri(dimethylsiloxy)phenylsilane dropwise, and continue to react for 11-13h. After the reaction is completed, cool to room temperature, remove the catalyst with silica gel, and finally perform reduced pressure distillation to remove toluene and unreacted boron-containing epoxy resin to obtain a boron-containing epoxy silicone monomer, wherein the amount ratio of boron-containing epoxy resin, toluene, catalyst and tri(dimethylsiloxy)phenylsilane is 95-105g:180-220mL:0.1-0.3g:55-65g.
[0024] In the above reaction process, phenylsilanetriol has silanol groups and dimethylchlorosilane has chlorine atoms. After the silanol groups on phenylsilanetriol are combined with the chlorine atoms on dimethylchlorosilane, tris(dimethylsiloxane)phenylsilane having a silicon-hydrogen bond is obtained; the boron-containing epoxy resin has a carbon-carbon double bond, which can be combined with the silicon-hydrogen bond on tris(dimethylsiloxane)phenylsilane through an addition reaction, and finally a boron-containing epoxy silicone monomer having an epoxy group is obtained.
[0025] Furthermore, the catalyst is a Karstedt catalyst.
[0026] Further, the boron-containing epoxy resin is prepared by the following steps:
[0027] Epichlorohydrin, polymerizable boric acid and benzyltriethylammonium chloride are reacted at 100-120°C for 1.5-2.5h, then a NaOH solution is added, and the reaction is continued for 4.5-5.5h, followed by washing with deionized water, and then unreacted epichlorohydrin is removed by vacuum distillation, and recrystallized in methanol for 2-3 times to obtain a boron-containing epoxy resin, wherein the NaOH solution refers to a NaOH solution with a concentration of 20wt%, and the amount ratio of epichlorohydrin, polymerizable boric acid, benzyltriethylammonium chloride and 20wt% NaOH solution is 345-355g:95-105g:3-4g:130-140g.
[0028] Further, the polymerizable boric acid is prepared by the following steps:
[0029] Under nitrogen protection, 10 mL of tetrahydrofuran and 0.87 g of Mg with the surface oxide layer removed were mixed, and then 3.92 mL of 4-bromostyrene dissolved in 20 mL of tetrahydrofuran was added at room temperature to obtain substance A. At the same time, 3.16 mL of bromobenzene dissolved in 30 mL of tetrahydrofuran was mixed with 0.87 g of Mg with the surface oxide layer removed under a nitrogen atmosphere, and stirred at room temperature for 2 hours to obtain bromobenzene Grignard reagent. Substance A and bromobenzene Grignard reagent were sequentially added dropwise to 3.34 mL of trimethyl borate and 20 mL of tetrahydrofuran at 0°C, and then stirred for 4 hours. After filtration, the mixture was extracted with a dichloromethane solution, and the upper organic solution was washed with a saturated aqueous ammonium chloride solution and deionized water for 3 times, and then the organic solution was dried with anhydrous sodium sulfate, concentrated under reduced pressure, and subjected to silica gel column chromatography with a petroleum ether / ethyl acetate mixture as an eluent to finally obtain polymerizable boronic acid.
[0030] A method for preparing a boron-modified silicone resin high temperature resistant coating comprises the following steps:
[0031] S1: Weigh the raw materials in the formula by mass, put the boron-modified silicone resin into the dispersion tank, adjust the speed to 400-500r / min, and seal and stir for 0.5-1.5h, then add the curing agent, film-forming agent, dispersant, thickener and hydroxyethyl cellulose, continue to seal and stir for 10-15min to obtain a premix;
[0032] S2: Grind the silicate filler fully and add it to the premix prepared in step S1 together with the composite inorganic pigment, adjust the rotation speed to 450-550r / min, and stir in a sealed state for 35-45min, control the temperature of the dispersion tank to be ≤45°C, detect the viscosity to be ≥95s, and the solid content to be ≥75%, and finally obtain a boron-modified silicone resin high temperature resistant coating.
[0033] Furthermore, the composite inorganic pigment is Yellow10C112 or Blue385 or Yellow29.
[0034] Furthermore, the silicate filler is one or more of talc powder, mica powder and kaolin.
[0035] Furthermore, the curing agent is one or more of diethylenetriamine, p-phenylenediamine, DMP-30, polyamide and triethylenetetramine.
[0036] Furthermore, the film-forming agent is propylene glycol methyl ether acetate and dipropylene glycol butyl ether, and the weight ratio of propylene glycol methyl ether acetate to dipropylene glycol butyl ether is 1:1.
[0037] The dispersant is one or more of sodium polyacrylate, fatty alcohol polyoxyethylene ether and ethylene bisstearamide.
[0038] The thickener is polyvinyl alcohol or polyacrylamide.
[0039] Beneficial effects of the present invention:
[0040] (1) In the technical scheme of the present invention, a boron-containing epoxy resin is prepared by combining epichlorohydrin with polymerizable boric acid. The boron element in the polymerizable boric acid can improve the high temperature resistance of the silicone resin. When the polymerizable boric acid is introduced into the silicone resin, a close-fitting network structure will be presented inside the silicone resin molecule, which also improves the weather resistance and mechanical properties of the coating. At the same time, the polymerizable boric acid also provides carbon-carbon double bonds and hydroxyl groups for subsequent reactions. A boron-containing epoxy silicone monomer is obtained by combining the boron-containing epoxy resin with tri(dimethylsiloxane)phenylsilane. The boron-containing epoxy silicone monomer not only provides epoxy groups for subsequent reactions, but also improves the heat resistance of tri(dimethylsiloxane)phenylsilane. The boron-containing epoxy silicone monomer is modified by a silane coupling agent and nanoparticles to obtain a modified silicone monomer. The silane coupling agent combines the nanoparticles with the boron-containing epoxy silicone monomer, thereby increasing the dispersibility and hydrophobicity of the nanoparticles in the boron-containing epoxy silicone monomer. At the same time, the nanoparticles also improve the mechanical properties and wear resistance of the boron-containing epoxy silicone monomer.
[0041] (2) In the technical scheme of the present invention, a boron-modified silicone resin is obtained by blending a rigid aromatic compound, a modified silicone monomer and a silicone resin. The rigid aromatic compound has a high-strength molecular structure and can enhance the structural rigidity of the silicone resin and improve the mechanical properties of the silicone resin. The nanoparticles in the modified silicone monomer act as a hydroxyl catalyst between the silicone resin and the rigid aromatic compound, further enhancing the high temperature resistance and mechanical properties of the silicone resin. The boron-modified silicone resin, a composite inorganic pigment, a silicate filler, a curing agent, a film-forming agent, a dispersant, a thickener and hydroxyethyl cellulose are uniformly mixed to obtain a boron-modified silicone resin high temperature resistant coating, which generally improves the high temperature resistance and mechanical properties of the coating.
[0042] (3) In the technical scheme of the present invention, a boron-containing epoxy resin is combined with tri(dimethylsiloxy)phenylsilane, and then modified with a silane coupling agent and nanoparticles to obtain a modified silicone monomer, which is then blended with a rigid aromatic compound and a silicone resin to finally obtain a boron-modified silicone resin high-temperature resistant coating. The prepared coating not only has good high-temperature resistance and mechanical properties, but also has good thermal stability. The coating has good adhesion at high temperatures and is not easy to discolor, crack or fall off. The overall performance of the coating is improved and its application range is expanded. DETAILED DESCRIPTION
[0043] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] The specific parameters of the raw materials used in the present invention are as follows:
[0045] Boron nitride particles with a particle size of 1 μm were purchased from Shanghai Meirui Chemical Technology Co., Ltd.; the diameter of carbon nanotubes was 2-20 nm; tetrahydrofuran was distilled from Na / benzophenone before use.
[0046] The polymerizable boric acid is prepared by the following steps:
[0047] Under nitrogen protection, 10 mL of tetrahydrofuran and 0.87 g of Mg with the surface oxide layer removed were mixed, and then 3.92 mL of 4-bromostyrene dissolved in 20 mL of tetrahydrofuran was added at room temperature to obtain substance A. At the same time, 3.16 mL of bromobenzene dissolved in 30 mL of tetrahydrofuran was mixed with 0.87 g of Mg with the surface oxide layer removed under a nitrogen atmosphere, and stirred at room temperature for 2 hours to obtain bromobenzene Grignard reagent. Substance A and bromobenzene Grignard reagent were sequentially added dropwise to 3.34 mL of trimethyl borate and 20 mL of tetrahydrofuran at 0°C, and then stirred for 4 hours. After filtration, it was extracted with 30 mL of dichloromethane solution with a mass concentration of 0.02 g / mL, and the upper organic solution was washed with saturated ammonium chloride aqueous solution and deionized water for 3 times respectively, and then the organic solution was dried with anhydrous sodium sulfate, concentrated under reduced pressure, and silica gel column chromatography was performed with a petroleum ether / ethyl acetate mixture (volume ratio of 10:1) as the eluent to finally obtain polymerizable boronic acid.
[0048] Methylphenyl silicone resin is prepared by the following steps:
[0049] 100 g of deionized water and 1 g of anion exchange resin D296R were mixed evenly, then heated to 85° C., 19.8 g of phenyltrimethoxysilane and 54.5 g of methylphenyldimethoxysilane were added, and stirring was continued at 85° C. for 2 h. The residual anion exchange resin D296R was removed by filtration, and then the residual deionized water was removed by reduced pressure distillation at -0.096 MPa and 100° C., and finally cooled to room temperature to obtain methylphenyl silicone resin.
[0050] Example 1
[0051] Boron-containing epoxy resin is prepared by the following steps:
[0052] 345g of epichlorohydrin, 95g of polymerizable boric acid and 3g of benzyltriethylammonium chloride were reacted at 100°C for 1.5h, and then 130g of 20wt% NaOH solution was added and the reaction was continued for 4.5h, then washed with deionized water, and then unreacted epichlorohydrin was removed by vacuum distillation, and recrystallized twice in 1L of methanol at 78°C to obtain a boron-containing epoxy resin.
[0053] Example 2
[0054] Boron-containing epoxy resin is prepared by the following steps:
[0055] 350g of epichlorohydrin, 100g of polymerizable boric acid and 3.5g of benzyltriethylammonium chloride were reacted at 110°C for 2h, and then 135g of 20wt% NaOH solution was added and the reaction was continued for 5h, then washed with deionized water, and then unreacted epichlorohydrin was removed by vacuum distillation, and recrystallized twice in 1L of methanol at 78°C to obtain a boron-containing epoxy resin.
[0056] Example 3
[0057] Boron-containing epoxy resin is prepared by the following steps:
[0058] 355g of epichlorohydrin, 105g of polymerizable boric acid and 4g of benzyltriethylammonium chloride were reacted at 120°C for 2.5h, and then 140g of 20wt% NaOH solution was added and the reaction was continued for 5.5h, then washed with deionized water, and then unreacted epichlorohydrin was removed by vacuum distillation, and recrystallized three times in 1L of methanol at 78°C to obtain a boron-containing epoxy resin.
[0059] Example 4
[0060] The boron-containing epoxy silicone monomer is prepared by the following steps:
[0061] A1: 4.5 g of phenylsilanetriol, 15.5 g of dimethylchlorosilane, 80 mL of toluene and 11 g of pyridine were mixed and stirred under reflux for 6 h. After filtering, the mixture was washed with deionized water for 3 times and dried over anhydrous magnesium sulfate. The solvent was then removed by rotary distillation and then vacuum distillation was performed to obtain tri(dimethylsiloxy)phenylsilane.
[0062] A2: 95 g of the boron-containing epoxy resin prepared in Example 1, 180 mL of toluene and 0.1 g of Karstedt's catalyst were mixed and reacted at 65° C. under nitrogen protection for 0.5 h, and then 55 g of tri(dimethylsiloxy)phenylsilane was added and the reaction was continued for 11 h. After the reaction was completed, the mixture was cooled to room temperature and the Karstedt's catalyst was removed with silica gel. Finally, reduced pressure distillation was performed to remove toluene and unreacted boron-containing epoxy resin to obtain a boron-containing epoxy silicone monomer.
[0063] Example 5
[0064] The boron-containing epoxy silicone monomer is prepared by the following steps:
[0065] A1: 5 g of phenylsilanetriol, 16 g of dimethylchlorosilane, 100 mL of toluene and 11.5 g of pyridine were mixed, stirred and refluxed for 7 h, filtered, washed with deionized water 4 times, dried over anhydrous magnesium sulfate, and then the solvent was removed by rotary distillation, followed by reduced pressure distillation to obtain tris(dimethylsiloxy)phenylsilane;
[0066] A2: 100 g of the boron-containing epoxy resin prepared in Example 2, 200 mL of toluene and 0.2 g of Karstedt's catalyst were mixed and reacted at 70° C. under nitrogen protection for 1 h, and then 60 g of tri(dimethylsiloxy)phenylsilane was added and the reaction was continued for 12 h. After the reaction was completed, the mixture was cooled to room temperature and the Karstedt's catalyst was removed with silica gel. Finally, reduced pressure distillation was performed to remove toluene and unreacted boron-containing epoxy resin to obtain a boron-containing epoxy silicone monomer.
[0067] Example 6
[0068] The boron-containing epoxy silicone monomer is prepared by the following steps:
[0069] A1: 5.5 g of phenylsilanetriol, 16.5 g of dimethylchlorosilane, 120 mL of toluene and 12 g of pyridine were mixed and stirred under reflux for 8 h. After filtering, the mixture was washed with deionized water for 5 times and dried over anhydrous magnesium sulfate. The solvent was then removed by rotary distillation and then vacuum distillation was performed to obtain tri(dimethylsiloxy)phenylsilane.
[0070] A2: 105 g of the boron-containing epoxy resin prepared in Example 3, 220 mL of toluene and 0.3 g of Karstedt's catalyst were mixed and reacted at 75° C. under nitrogen protection for 1.5 h, and then 65 g of tri(dimethylsiloxy)phenylsilane was added and the reaction was continued for 13 h. After the reaction was completed, the mixture was cooled to room temperature and the Karstedt's catalyst was removed with silica gel. Finally, reduced pressure distillation was performed to remove toluene and unreacted boron-containing epoxy resin to obtain a boron-containing epoxy silicone monomer.
[0071] Comparative Example 1
[0072] The difference between this comparative example and Example 5 is that the mass of the boron-containing epoxy resin prepared in Example 2 is replaced by polymerizable boric acid, and the remaining steps and raw materials are the same as those in Example 5.
[0073] Comparative Example 2
[0074] The difference between this comparative example and Example 5 is that in this comparative example, the mass of the boron-containing epoxy resin is replaced by tri(dimethylsiloxy)phenylsilane, and the remaining steps and raw materials are the same as those in Example 5.
[0075] Comparative Example 3
[0076] The difference between this comparative example and Example 5 is that in this comparative example, the mass of tri(dimethylsiloxy)phenylsilane is replaced by boron-containing epoxy resin, and the remaining steps and raw materials are synchronized with Example 5.
[0077] Example 7
[0078] The modified silicone monomer is prepared by the following steps:
[0079] 0.8 g of boron nitride particles, 2.8 g of KH550 and 140 mL of 95% ethanol solution were mixed evenly, and then stirred for 2 h under a nitrogen atmosphere at 50 ° C., and then 18 g of the boron-containing epoxy silicone monomer prepared in Example 4 was added, and the reaction was continued for 2 h, and then heated to 85 ° C. to remove ethanol, and finally cooled to room temperature to obtain a modified silicone monomer.
[0080] Example 8
[0081] The modified silicone monomer is prepared by the following steps:
[0082] 1 g of boron nitride particles, 3 g of KH550 and 150 mL of 95% ethanol solution were mixed evenly, and then stirred for 3 h under a nitrogen atmosphere at 60° C., and then 20 g of the boron-containing epoxy silicone monomer prepared in Example 5 was added, and the reaction was continued for 3 h, and then heated to 90° C. to remove ethanol, and finally cooled to room temperature to obtain a modified silicone monomer.
[0083] Example 9
[0084] The modified silicone monomer is prepared by the following steps:
[0085] 1.2 g of carbon nanotubes, 3.2 g of KH550 and 160 mL of 95% ethanol solution were mixed evenly, and then stirred for 4 h under a nitrogen atmosphere at 70° C., and then 22 g of the boron-containing epoxy silicone monomer prepared in Example 6 was added, and the reaction was continued for 4 h, and then heated to 95° C. to remove ethanol, and finally cooled to room temperature to obtain a modified silicone monomer.
[0086] Comparative Example 4
[0087] The difference between this comparative example and Example 8 is that the boron-containing epoxy silicone monomer prepared in Example 5 is replaced by the substance prepared in Comparative Example 1, and the remaining steps and raw materials are the same as in Example 8.
[0088] Comparative Example 5
[0089] The difference between this comparative example and Example 8 is that the boron-containing epoxy silicone monomer prepared in Example 5 is replaced by the substance prepared in Comparative Example 2, and the remaining steps and raw materials are the same as in Example 8.
[0090] Comparative Example 6
[0091] The difference between this comparative example and Example 8 is that the boron-containing epoxy silicone monomer prepared in Example 5 is replaced by the substance prepared in Comparative Example 3, and the remaining steps and raw materials are the same as in Example 8.
[0092] Example 10
[0093] Boron-modified silicone resin is prepared by the following steps:
[0094] 0.8 g of 3-hydroxy-1,2,3-benzotriazine-4(3H)-one was dissolved in 20 mL of ethanol, and then 0.8 g of the modified silicone monomer prepared in Example 7 and 3.8 g of methylphenyl silicone resin were added, and stirred at 70° C. for 6 h. After filtering, the mixture was washed with deionized water, and then distilled under reduced pressure at 120° C. for 1 h. Finally, it was cooled to room temperature to obtain a boron-modified silicone resin.
[0095] Embodiment 11
[0096] Boron-modified silicone resin is prepared by the following steps:
[0097] 1 g of 3-hydroxy-1,2,3-benzotriazine-4(3H)-one was dissolved in 25 mL of ethanol, and then 1 g of the modified silicone monomer prepared in Example 8 and 4 g of methylphenyl silicone resin were added, and stirred at 80° C. for 7 h. After filtering, the mixture was washed with deionized water, and then distilled under reduced pressure at 130° C. for 1.5 h. Finally, the mixture was cooled to room temperature to obtain a boron-modified silicone resin.
[0098] Example 12
[0099] Boron-modified silicone resin is prepared by the following steps:
[0100] 1.2 g of 3-hydroxy-1,2,3-benzotriazine-4(3H)-one was dissolved in 30 mL of ethanol, and then 1.2 g of the modified silicone monomer prepared in Example 9 and 4.2 g of methylphenyl silicone resin were added, and stirred at 90° C. for 8 h. After filtering, the mixture was washed with deionized water, and then distilled under reduced pressure at 140° C. for 2 h. Finally, it was cooled to room temperature to obtain a boron-modified silicone resin.
[0101] Comparative Example 7
[0102] The difference between this comparative example and Example 11 is that the modified organosilicon monomer prepared in Example 8 is replaced by the substance prepared in Comparative Example 4, and the remaining steps and raw materials are the same as Example 11.
[0103] Comparative Example 8
[0104] The difference between this comparative example and Example 11 is that the modified organosilicon monomer prepared in Example 8 is replaced by the substance prepared in Comparative Example 5, and the remaining steps and raw materials are the same as Example 11.
[0105] Comparative Example 9
[0106] The difference between this comparative example and Example 11 is that the modified organosilicon monomer prepared in Example 8 is replaced by the substance prepared in Comparative Example 6, and the remaining steps and raw materials are the same as Example 11.
[0107] Comparative Example 10
[0108] The difference between this comparative example and Example 11 is that the modified silicone monomer prepared in Example 8 is replaced by the boron-containing epoxy silicone monomer prepared in Example 5, and the remaining steps and raw materials are the same as in Example 11.
[0109] Comparative Example 11
[0110] The difference between this comparative example and Example 11 is that the boron-modified silicone resin is prepared without adding a rigid aromatic compound.
[0111] Comparative Example 12
[0112] The difference between this comparative example and Example 11 is that the boron-modified organic silicone resin is prepared without adding modified organic silicone monomer.
[0113] Embodiment 13
[0114] A boron-modified silicone resin high-temperature resistant coating comprises the following raw materials in parts by weight: 35 parts of the boron-modified silicone resin prepared in Example 10, 8 parts of Yellow 10C112, 5 parts of talc, 12 parts of diethylenetriamine, 2 parts of propylene glycol methyl ether acetate, 2 parts of dipropylene glycol butyl ether, 3 parts of sodium polyacrylate, 4 parts of polyvinyl alcohol and 3 parts of hydroxyethyl cellulose.
[0115] The following steps are involved:
[0116] S1: Weigh the raw materials by weight of the formula, put the boron-modified silicone resin prepared in Example 10 into a dispersion tank, adjust the speed to 400 r / min, and seal and stir for 0.5 h, then add diethylenetriamine, propylene glycol methyl ether acetate, dipropylene glycol butyl ether, sodium polyacrylate, polyvinyl alcohol and hydroxyethyl cellulose, continue to seal and stir for 10 min to obtain a premix;
[0117] S2: Grind talcum powder to a particle size of 5 μm and add it to the premix prepared in step S1 with Yellow 10C112. Adjust the rotation speed to 450 r / min, seal and stir for 35 min, control the temperature of the dispersion tank to 40°C, detect the viscosity for 100 s, and obtain a boron-modified silicone resin high temperature resistant coating.
[0118] Embodiment 14
[0119] A boron-modified silicone resin high-temperature resistant coating comprises the following raw materials in parts by weight: 40 parts of the boron-modified silicone resin prepared in Example 11, 10 parts of Blue 385, 8 parts of mica powder, 14 parts of p-phenylenediamine, 2 parts of propylene glycol methyl ether acetate, 3 parts of dipropylene glycol butyl ether, 4 parts of fatty alcohol polyoxyethylene ether, 5 parts of polyvinyl alcohol and 4 parts of hydroxyethyl cellulose.
[0120] The following steps are involved:
[0121] S1: Weigh the raw materials by weight of the formula, put the boron-modified silicone resin prepared in Example 11 into a dispersion tank, adjust the speed to 450 r / min, and seal and stir for 1 hour, then add p-phenylenediamine, propylene glycol methyl ether acetate, dipropylene glycol butyl ether, fatty alcohol polyoxyethylene ether, polyvinyl alcohol and hydroxyethyl cellulose, continue to seal and stir for 13 minutes to obtain a premix;
[0122] S2: Grind the mica powder fully to a particle size of 5 μm and add it to the premix prepared in step S1 with Blue 385, adjust the rotation speed to 500 r / min, seal and stir for 40 min, control the temperature of the dispersion tank to 40°C, detect the viscosity for 100 s, and obtain a boron-modified silicone resin high temperature resistant coating.
[0123] Embodiment 15
[0124] A boron-modified silicone resin high-temperature resistant coating comprises the following raw materials in parts by weight: 45 parts of the boron-modified silicone resin prepared in Example 12, 12 parts of Yellow 29, 10 parts of kaolin, 15 parts of polyamide, 3 parts of propylene glycol methyl ether acetate, 3 parts of dipropylene glycol butyl ether, 5 parts of ethylene bisstearamide, 6 parts of polyacrylamide and 5 parts of hydroxyethyl cellulose.
[0125] The following steps are involved:
[0126] S1: Weigh the raw materials by weight of the formula, put the boron-modified silicone resin prepared in Example 12 into a dispersion tank, adjust the speed to 500 r / min, and seal and stir for 1.5 hours, then add polyamide, propylene glycol methyl ether acetate, dipropylene glycol butyl ether, ethylene bisstearamide, polyacrylamide and hydroxyethyl cellulose, continue to seal and stir for 15 minutes to obtain a premix;
[0127] S2: Grind kaolin fully to a particle size of 5 μm and add it to the premix prepared in step S1 with Yellow 29, adjust the rotation speed to 550 r / min, seal and stir for 45 min, control the temperature of the dispersion tank to 40° C., detect the viscosity for 100 s, and obtain a boron-modified silicone resin high temperature resistant coating.
[0128] Comparative Example 13
[0129] The difference between this comparative example and Example 14 is that the boron-modified silicone resin prepared in Example 11 is replaced by the material prepared in Comparative Example 7, and the remaining steps and raw materials are the same as those in Example 14.
[0130] Comparative Example 14
[0131] The difference between this comparative example and Example 14 is that the boron-modified silicone resin prepared in Example 11 is replaced by the material prepared in Comparative Example 8, and the remaining steps and raw materials are the same as those in Example 14.
[0132] Comparative Example 15
[0133] The difference between this comparative example and Example 14 is that the boron-modified silicone resin prepared in Example 11 is replaced by the material prepared in Comparative Example 9, and the remaining steps and raw materials are the same as those in Example 14.
[0134] Comparative Example 16
[0135] The difference between this comparative example and Example 14 is that the boron-modified silicone resin prepared in Example 11 is replaced by the material prepared in Comparative Example 10, and the remaining steps and raw materials are the same as Example 14.
[0136] Comparative Example 17
[0137] The difference between this comparative example and Example 14 is that the boron-modified silicone resin prepared in Example 11 is replaced by the substance prepared in Comparative Example 11, and the remaining steps and raw materials are the same as Example 14.
[0138] Comparative Example 18
[0139] The difference between this comparative example and Example 14 is that the boron-modified silicone resin prepared in Example 11 is replaced by the material prepared in Comparative Example 12, and the remaining steps and raw materials are the same as those in Example 14.
[0140] Comparative Example 19
[0141] The difference between this comparative example and Example 14 is that the mass of the boron-modified silicone resin is replaced by methylphenyl silicone resin, and the remaining steps and raw materials are the same as Example 14.
[0142] The boron-modified silicone resin high temperature resistant coatings prepared in Examples 13-15 and Comparative Examples 13-19 are tested. The boron-modified silicone resin high temperature resistant coatings are coated on a thin steel plate with a size of 5*120*1 mm. The thin steel plate is degreased and derusted to ensure that the surface is clean and dry. After being cured at room temperature for 24 hours, relevant performance tests are performed. The high temperature resistance is tested according to GB / T 1735-89, the storage stability and adhesion are tested according to GB / T 1720-89, and the impact strength is tested according to GB / T1732-1993. The test results are shown in the following table:
[0143] Table 1
[0144]
[0145]
[0146] It can be seen from the data in Table 1 above that, by comparing Comparative Example 13 with Example 14, it can be seen that the test results of the silicone monomer prepared by combining polymerizable boric acid with tri(dimethylsiloxane)phenylsilane are worse than those of Example 11, indicating that combining epichlorohydrin with polymerizable boric acid and then reacting with tri(dimethylsiloxane)phenylsilane to prepare a boron-containing epoxy silicone monomer can increase the adhesion performance of the boron-containing epoxy silicone monomer and enhance the heat resistance of the boron-containing epoxy silicone monomer;
[0147] From the comparison of Comparative Examples 14-15 and Example 14, it can be seen that the high temperature resistant coating is prepared by not adding the boron-containing epoxy resin or not adding tri(dimethylsiloxane)phenylsilane, indicating that the combination of tri(dimethylsiloxane)phenylsilane and the boron-containing epoxy resin can improve the heat resistance and adhesion of the boron-containing epoxy silicone monomer, and further improve the high temperature resistance and mechanical properties of the coating;
[0148] From the comparison between Comparative Example 16 and Example 14, it can be seen that the modified silicone monomer is prepared using the boron-containing epoxy silicone monomer, which indicates that the boron-containing epoxy silicone monomer is combined with nanoparticles and a silane coupling agent to increase the dispersibility of the nanoparticles and further improve the mechanical properties and heat resistance of the coating.
[0149] From the comparison of Comparative Examples 17-18 and Example 14, it can be seen that the high temperature resistant coating is prepared without adding rigid aromatic compounds or modified silicone monomers, which indicates that the high temperature resistance and mechanical properties of the silicone resin can be increased by blending rigid aromatic compounds, modified silicone monomers and silicone resins to obtain boron-modified silicone resins.
[0150] From the comparison between Comparative Example 19 and Example 14, it can be seen that the mechanical strength, heat resistance and adhesion properties of the high-temperature resistant coating prepared by using methylphenyl silicone resin are worse than those of Example 14, indicating that the coating prepared by adding boron-modified silicone resin has better mechanical properties, high-temperature resistance and adhesion properties.
[0151] It can be seen from Table 1 above that the boron-modified silicone resin high temperature resistant coating prepared in Examples 13-15 is compared with Comparative Examples 13-19. The boron-containing epoxy resin is combined with tri(dimethylsiloxy)phenylsilane, and then modified with a silane coupling agent and nanoparticles to obtain a modified silicone monomer, which is then blended with a rigid aromatic compound and a silicone resin to obtain a boron-modified silicone resin high temperature resistant coating. The mechanical properties and high temperature resistance of the coating are increased and the test performance requirements are met. The boron-modified silicone resin high temperature resistant coating prepared in Comparative Examples 13-19 did not meet the performance requirements. The boron-modified silicone resin high temperature resistant coating prepared by the present invention not only has good high temperature resistance and mechanical properties, but also has good adhesion and thermal stability, which greatly improves the comprehensive performance of the coating.
[0152] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0153] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A boron-modified silicone resin high temperature resistant coating, characterized in that: The invention comprises the following raw materials in parts by weight: 35-45 parts of boron-modified organic silicon resin, 8-12 parts of composite inorganic pigment, 5-10 parts of silicate filler, 12-15 parts of curing agent, 4-6 parts of film-forming agent, 3-5 parts of dispersant, 4-6 parts of thickener and 3-5 parts of hydroxyethyl cellulose; The boron-modified silicone resin is prepared by blending a rigid aromatic compound, a modified silicone monomer and a silicone resin; the modified silicone monomer is prepared by modifying a boron-containing epoxy silicone monomer with a silane coupling agent and nanoparticles; the boron-containing epoxy silicone monomer is prepared by combining a boron-containing epoxy resin with tris(dimethylsiloxy)phenylsilane; the boron-containing epoxy resin is prepared by combining epichlorohydrin with polymerizable boric acid; The modified organosilicon monomer is prepared by the following steps: The nanoparticles, silane coupling agent and ethanol solution are mixed evenly, and then stirred for 2-4 hours at 50-70° C. in a nitrogen atmosphere, and then the boron-containing epoxy silicone monomer is added and the reaction is continued for 2-4 hours, and then heated to 85-95° C. to remove ethanol, and finally cooled to room temperature to obtain a modified silicone monomer; The boron-containing epoxy silicone monomer is prepared by the following steps: A1: Phenylsilanetriol, dimethylchlorosilane, toluene and pyridine are mixed and stirred under reflux for 6-8 hours. After filtering, the mixture is washed with deionized water for 3-5 times, dried with anhydrous magnesium sulfate, and then subjected to rotary distillation and reduced pressure distillation to obtain tris(dimethylsiloxy)phenylsilane; A2: Mix the boron-containing epoxy resin, toluene and catalyst, and react at 65-75°C under nitrogen protection for 0.5-1.5h, then dropwise add tri(dimethylsiloxy)phenylsilane, and continue to react for 11-13h. After the reaction is completed, cool to room temperature, and finally perform reduced pressure distillation to obtain a boron-containing epoxy silicone monomer; The boron-containing epoxy resin is prepared by the following steps: Epichlorohydrin, polymerizable boric acid and benzyltriethylammonium chloride are reacted at 100-120° C. for 1.5-2.5 hours, then a NaOH solution is added, and the reaction is continued for 4.5-5.5 hours, and then washed with deionized water, and then vacuum distilled, and recrystallized in methanol for 2-3 times to obtain a boron-containing epoxy resin; The polymerizable boronic acid is prepared by the following steps: Under nitrogen protection, 10 mL of tetrahydrofuran and 0.87 g of Mg with the surface oxide layer removed were mixed, and then 3.92 mL of 4-bromostyrene dissolved in 20 mL of tetrahydrofuran was added at room temperature to obtain substance A. At the same time, 3.16 mL of bromobenzene dissolved in 30 mL of tetrahydrofuran was mixed with 0.87 g of Mg with the surface oxide layer removed under a nitrogen atmosphere, and stirred at room temperature for 2 hours to obtain bromobenzene Grignard reagent. Substance A and bromobenzene Grignard reagent were sequentially added dropwise to 3.34 mL of trimethyl borate and 20 mL of tetrahydrofuran at 0°C, and then stirred for 4 hours. After filtration, the mixture was extracted with a dichloromethane solution, and the upper organic solution was washed with a saturated aqueous ammonium chloride solution and deionized water for 3 times, and then the organic solution was dried with anhydrous sodium sulfate, concentrated under reduced pressure, and subjected to silica gel column chromatography with a petroleum ether / ethyl acetate mixture as an eluent to finally obtain polymerizable boronic acid.
2. The boron-modified silicone resin high temperature resistant coating according to claim 1, characterized in that: The boron-modified organosilicon resin is prepared by the following steps: The rigid aromatic compound is dissolved in ethanol, and then the modified silicone monomer and silicone resin are added, and stirred at 70-90°C for 6-8h. After filtering, it is washed with deionized water, and then distilled under reduced pressure at 120-140°C for 1-2h, and finally cooled to room temperature to obtain a boron-modified silicone resin.
3. The boron-modified silicone resin high temperature resistant coating according to claim 2, characterized in that: The usage ratio of the rigid aromatic compound, ethanol, modified silicone monomer and modified silicone resin is 0.8-1.2g:20-30mL:0.8-1.2g:3.8-4.2g.
4. The boron-modified silicone resin high temperature resistant coating according to claim 2, characterized in that: The rigid aromatic compound is 3-hydroxy-1,2,3-benzotriazine-4(3H)-one.
5. The boron-modified silicone resin high temperature resistant coating according to claim 1, characterized in that: The usage ratio of the nanoparticles, the silane coupling agent, the ethanol solution and the boron-containing epoxy silicone monomer is 0.8-1.2 g: 2.8-3.2 g: 140-160 mL: 18-22 g.
6. The boron-modified silicone resin high temperature resistant coating according to claim 1, characterized in that: The nanoparticles are boron nitride particles or carbon nanotubes.
7. A method for preparing a boron-modified silicone resin high temperature resistant coating according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: Weigh the raw materials in the formula by mass, put the boron-modified silicone resin into the dispersion tank, adjust the speed to 400-500r / min, and seal and stir for 0.5-1.5h, then add the curing agent, film-forming agent, dispersant, thickener and hydroxyethyl cellulose, continue to seal and stir for 10-15min to obtain a premix; S2: Grind the silicate filler thoroughly and add it to the premix prepared in step S1 together with the composite inorganic pigment, adjust the rotation speed to 450-550r / min, and stir in a sealed state for 35-45min, control the temperature of the dispersion cylinder to be ≤45°C, detect the viscosity to be ≥95s, and the solid content to be ≥75%, and finally obtain a boron-modified silicone resin high temperature resistant coating.
Citation Information
Cited By
Organic silicon inorganic modified resin as well as preparation method and application thereof
CN120098537A