A perovskite battery and a method for preparing the same
By setting an interface passivation layer between the perovskite light-absorbing layer and the electron-transporting layer, the problem of insufficient adhesion between the light-absorbing layer and the electron-transporting layer in the perovskite battery is solved, and the battery's long life and high conversion efficiency are achieved.
Patent Information
- Application Number
- CN202410931410.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The adhesion between the perovskite light-absorbing layer and the fullerene electron transport layer in trans-perovskite solar cells is weak, resulting in delamination, shortened service life, and low conversion efficiency.
An interface passivation layer is set between the perovskite light absorption layer and the electron transport layer. 3,5-bis(carboxylic acid)-phenyl-3-maleimide is used as the interface passivation agent to bond with the perovskite through chemical bonds. The mineral surface is connected and assembled with fullerene and its derivatives to achieve molecular layer assembly, locking the electron transport layer and preventing it from falling off.
It extends the service life of perovskite batteries, improves conversion efficiency, and enhances battery stability and performance.
Smart Images

Figure CN118475140B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar cells, and in particular relates to a perovskite cell and a preparation method thereof. Background Art
[0002] Organic-inorganic hybrid lead halide perovskite cells (PSCs) have attracted extensive attention due to their advantages such as low cost, high efficiency, low electron-hole recombination rate, long carrier migration length and large absorption cross-section area.
[0003] In inverse perovskite solar cells, there is very weak adhesion between the perovskite light-absorbing layer and the fullerene and its derivative electron-transporting layer, which may lead to delamination and thus greatly shorten the operating life of PSCs.
[0004] Therefore, developing a perovskite battery with good adhesion between the perovskite light absorption layer and the fullerene and its derivative electron transport layer, not easy to fall off, long service life and high conversion efficiency is an urgent problem to be solved in this field. Summary of the invention
[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a perovskite battery and a preparation method thereof. The perovskite battery can realize molecular layer assembly with the fullerene and its derivative electron transport layer by setting a specific interface passivation layer between the perovskite light absorption layer and the electron transport layer, so that it is not easy to fall off, thereby extending the service life of the battery, and can also passivate the defects of the perovskite light absorption layer, improve the conversion efficiency and further enhance the service life of the perovskite battery.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a perovskite battery, wherein an interface passivation layer is arranged between the perovskite light absorption layer and the electron transport layer of the perovskite battery; the raw material of the interface passivation layer includes 3,5-di(carboxylic acid)-phenyl-3-maleimide; the electron transport layer includes fullerene and its derivative electron transport layer; the interface passivation layer is connected to the perovskite light absorption layer and the electron transport layer by chemical bonds.
[0008] In the present invention, 3,5-di(carboxylic acid)-phenyl-3-maleimide (BCPM, C 12 H7NO6) as an interface passivator, the maleimide group on it is rotated 35 degrees relative to the horizontal direction of the surface, and the oxygen and halogen ions on one side have significant charge transfer, forming ionic bonds, anchoring the molecule to the perovskite surface, and the carbonyl group can react with uncoordinated metal ions (such as Pb 2+) interaction, repairing the vacancy defects of halogen (such as I), 3,5-di(carboxylic acid)-phenyl-3-maleimide can be surface synthesized (OSS) on the perovskite surface, and the interface passivator molecules are orderly self-assembled and locked on the perovskite surface; at the same time, fullerene and its derivatives are stacked on BCPM to realize molecular layer assembly, so that the lowest unoccupied orbital of fullerene and its derivatives and the highest occupied orbital of BCPM match, and through the cycloaddition reaction between molecular layers ([2+2] cycloaddition between fullerene and its derivative molecules and [2+4] cycloaddition between fullerene and its derivative molecules and interface passivator), the precursor molecules are bonded perpendicular to the surface direction, locking the fullerene and its derivatives, making them not easy to fall off, quickly transmitting carriers, enhancing the service life of the perovskite battery and improving the conversion efficiency of the perovskite battery.
[0009] In the present invention, the fullerene and its derivatives include C 20 , C 60 , C 70 , C 76 , C 80 At least one of .
[0010] In the present invention, the thickness of the interface passivation layer is 1~10 nm, for example, it can be 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, 5.5 nm, 6 nm, 6.5 nm, 7 nm, 7.5 nm, 8 nm, 8.5 nm, 9 nm, 9.5 nm, 10 nm, etc.
[0011] In the present invention, when the thickness of the interface passivation layer is within the above-defined range, the conversion efficiency of the obtained perovskite battery is higher; more preferably, the thickness is 4 to 6 nm.
[0012] In the present invention, the general structural formula of the material of the perovskite light-absorbing layer is ABX3.
[0013] Wherein, A is selected from CH3NH3 + 、CH(NH2)2 + , Rb + or Cs + Any one or a combination of at least two of the following: B is selected from Pb 2+ ,Ge 2+ Sn 2+ Any one or a combination of at least two of, X is selected from Cl - Br - or I - Any one or a combination of at least two of the following.
[0014] In the present invention, the thickness of the perovskite light absorbing layer is 400-700 nm, for example, it can be 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, etc.
[0015] In the present invention, the thickness of the fullerene and its derivative electron transport layer is 10-30 nm, for example, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, 20 nm, 22 nm, 24 nm, 26 nm, 28 nm, 30 nm, etc.
[0016] In the present invention, the side of the fullerene and its derivative electron transport layer away from the interface passivation layer is also provided with SnO x Electron transport layer; the SnO x The thickness of the electron transport layer is 5 to 20 nm, for example, 5 nm, 6 nm, 8 nm, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, 20 nm, etc.
[0017] In the present invention, the SnO x Including SnO2.
[0018] In the present invention, a hole transport layer is sequentially arranged on the side of the perovskite light absorption layer away from the interface passivation layer.
[0019] In the present invention, the material of the hole transport layer includes nickel oxide and / or [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid (MeO-2PACz).
[0020] In the present invention, the thickness of the hole transport layer is 10-20 nm, for example, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, 20 nm, etc.
[0021] In the present invention, the perovskite cell includes a single-junction perovskite solar cell and / or a perovskite crystalline silicon stacked cell.
[0022] In the present invention, a conductive glass substrate is further provided on the side of the hole transport layer of the single-junction perovskite solar cell away from the perovskite light absorption layer.
[0023] In the present invention, the conductive glass substrate includes any one of an indium tin oxide conductive glass substrate (ITO conductive glass substrate), a fluorine-doped SnO2 conductive glass substrate (FTO conductive glass substrate) or an aluminum-doped ZnO conductive glass substrate (AZO conductive glass substrate).
[0024] In the present invention, an electrode is further provided on a side of the electron transport layer of the single-junction perovskite solar cell away from the interface passivation layer.
[0025] In the present invention, the electrode comprises a metal electrode; the thickness of the metal electrode is 80-150 nm, for example, it can be 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, etc.
[0026] In the present invention, a composite layer and a crystalline silicon cell substrate are sequentially arranged on the side of the hole transport layer of the perovskite crystalline silicon stacked cell away from the perovskite light absorption layer.
[0027] In the present invention, the crystalline silicon cell substrate comprises a back conductive metal electrode, a back transparent conductive layer, a p-type amorphous silicon layer, a first intrinsic amorphous silicon layer, a silicon wafer, a second intrinsic amorphous silicon layer and an n-type amorphous silicon layer stacked in sequence; the n-type amorphous silicon layer is stacked with a composite layer.
[0028] In the present invention, the composite layer includes at least one of an indium tin oxide composite layer, a fluorine-doped SnO2 composite layer or an aluminum-doped ZnO composite layer; the thickness of the composite layer is 20~40 nm, for example, it can be 20 nm, 22 nm, 24 nm, 26nm, 28 nm, 30 nm, 32 nm, 34 nm, 36 nm, 38 nm, 40 nm, etc.
[0029] In the present invention, an electrode is further provided on the side of the electron transport layer of the perovskite crystalline silicon stacked cell away from the interface passivation layer; the electrode comprises a metal electrode; the thickness of the metal electrode is 800~1000 nm, for example, it can be 800 nm, 820 nm, 840 nm, 860 nm, 880 nm, 900 nm, 920 nm, 940 nm, 960 nm, 980 nm, 1000 nm, etc.
[0030] In the present invention, in the perovskite crystalline silicon stacked cell, a conductive layer is further provided between the electron transport layer and the electrode.
[0031] In the present invention, the material of the conductive layer includes at least one of indium tin oxide, fluorine-doped SnO2 or aluminum-doped ZnO; the thickness of the conductive layer is 80~140 nm, for example, it can be 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, etc.
[0032] In a second aspect, the present invention provides a method for preparing a perovskite battery according to the first aspect, the preparation method comprising the following steps:
[0033] The raw materials of the interface passivation layer and fullerene and its derivatives are sequentially deposited on the surface of the perovskite light absorption layer, and annealed to obtain the interface passivation layer connected to the perovskite light absorption layer and the electron transport layer through chemical bonds.
[0034] Preferably, the deposition method comprises evaporation; the deposition rate is 0.01-0.05 nm / s, for example, 0.01 nm / s, 0.015 nm / s, 0.02 nm / s, 0.025 nm / s, 0.03 nm / s, 0.035 nm / s, 0.04 nm / s, 0.045 nm / s, 0.05 nm / s, etc.
[0035] The annealing temperature is 80-120°C, for example, it can be 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C, 100°C, 102°C, 105°C, 108°C, 110°C, 112°C, 115°C, 118°C, 120°C, etc.; the annealing time is 3-15 min, for example, it can be 5 min, 5.5 min, 6 min, 6.5 min, 7 min, 7.5 min, 8 min, 8.5min, 9 min, 9.5 min, 10 min, 10.5 min, 11 min, 11.5 min, 12 min, 12.5 min, 13 min, 13.5min, 14 min, 14.5 min, 15 min, etc.
[0036] In the present invention, in the preparation method, annealing is performed after the raw materials of the interface passivation layer and fullerene and its derivatives are sequentially deposited on the surface of the perovskite light-absorbing layer, so that the interface passivator and the fullerene and its derivative molecules can realize intermolecular [4+2] cycloaddition reaction and [2+2] cycloaddition reaction, thereby realizing self-assembly of the molecular layer, avoiding the stratification of the perovskite light-absorbing layer and the fullerene and its derivative electron transport layer, and improving the conversion efficiency of the service life of the perovskite battery; and when the temperature and time of the annealing are within the above-defined range, the perovskite battery has a longer service life and a higher conversion efficiency.
[0037] In the present invention, the preparation method of the hole transport layer includes a magnetron sputtering method and / or a solution method; when the material of the hole transport layer includes nickel oxide and [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid, the preparation method includes: depositing nickel oxide on the surface of a substrate by a magnetron sputtering method to obtain a nickel oxide layer; then coating the surface of the nickel oxide layer with a [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid solution (with a concentration of 0.5-1.5 mM, and the solvent includes but is not limited to methanol), the coating speed is 2000-4000 rad / s, and then annealing at 80-120°C for 5-15 min to obtain the hole transport layer.
[0038] In the present invention, the preparation method of the perovskite light absorbing layer includes an atomic layer deposition method or a solution method.
[0039] In the present invention, the preparation method of the electrode includes an evaporation method.
[0040] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] The perovskite battery provided by the present invention can realize molecular layer assembly with the electron transport layer of fullerene and its derivatives by setting a specific interface passivation layer between the perovskite light absorbing layer and the electron transport layer, so that it is not easy to fall off, thereby extending the service life of the battery, and can also self-assemble and lock in an orderly manner on the perovskite surface, passivate the defects of the perovskite light absorbing layer, improve the conversion efficiency and further enhance the service life of the perovskite battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 C in the present invention 60 Intermolecular [2+2] cycloaddition reaction and interfacial passivation agent and C 60 Schematic diagram of the [4+2] cycloaddition reaction between molecular layers;
[0044] Figure 2 In the perovskite battery provided by the present invention, the perovskite light absorption layer, the interface passivation layer and the C 60 Schematic diagram of the bonding structure of the electron transport layer;
[0045] Among them, 1-C 60 Electron transport layer; 2-interface passivation layer; 3-perovskite light absorption layer;
[0046] Figure 3 A schematic diagram of the structure of a perovskite battery provided in Example 1 of the present invention;
[0047] Among them, 100 is an ITO conductive glass substrate; 101 is a nickel oxide hole transport layer; 102 is a MeO-2PACz hole transport layer; 103 is a perovskite light absorption layer; 104 is an interface passivation layer; 105 is a C 60 Electron transport layer; 106 is a SnO2 electron transport layer; 107 is a conductive metal electrode.
[0048] Figure 4 A schematic diagram of the structure of a perovskite crystalline silicon tandem battery provided in Example 7 of the present invention;
[0049] Among them, 100 is a back conductive metal electrode; 101 is a back transparent conductive layer; 102 is a p-type amorphous silicon layer; 103 is a first intrinsic amorphous silicon layer; 104 is a silicon wafer; 105 is a second intrinsic amorphous silicon layer; 106 is an n-type amorphous silicon layer; 107 is a composite layer; 108 is a nickel oxide hole transport layer; 109 is a MeO-2PACz hole transport layer; 110 is a perovskite light absorption layer; 111 is an interface passivation layer; 112 is a C 60 Electron transport layer; 113 is a tin dioxide electron transport layer; 114 is a front transparent conductive layer; 115 is a front conductive metal electrode.
[0050] Figure 5 This is a curve chart showing changes in conversion efficiency of the perovskite cells provided in Example 2 of the present invention and Comparative Example 1 over time. DETAILED DESCRIPTION
[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0052] Example 1
[0053] This embodiment provides a perovskite solar cell, and its structural schematic diagram is as follows Figure 3 As shown; comprising sequentially stacked indium tin oxide conductive glass substrate (ITO glass substrate) 100, nickel oxide hole transport layer 101, MeO-2PACz hole transport layer 102, CsPbI3 perovskite light absorption layer 103, interface passivation layer 104, C 60 An electron transport layer 105, a tin dioxide electron transport layer 106 and a silver metal electrode 107; The method for preparing the perovskite solar cell comprises the following steps:
[0054] (1) After ultrasonic cleaning of ITO glass with glass cleaner, deionized water, ethanol, acetone, isopropanol, and ethanol for 15 min, the substrate was blown dry with dry air and then treated with UV-ozone for 20 min to obtain a cleaned ITO glass substrate.
[0055] (2) A layer of nickel oxide with a thickness of 15 nm is sputtered on the surface of the ITO glass substrate obtained in step (1) by a magnetron sputtering method to obtain a nickel oxide hole transport layer.
[0056] (3) Spin-coat the surface of the nickel oxide hole transport layer obtained in step (2) with a MeO-2PACz solution (the solvent is methanol and the concentration is 1 mM) at a spin-coating speed of 3000 rad / s; then anneal at 100°C for 10 min to obtain a MeO-2PACz hole transport layer with a thickness of 5 nm.
[0057] (4) A perovskite precursor 1 is deposited on the surface of the MeO-2PACz hole transport layer obtained in step (3) by atomic deposition technology. The perovskite precursor 1 includes cesium bis(trimethylsilyl)amide (Cs(btsa)) and tin(IV) iodide (SnI4). The deposition temperature is 150°C and the deposition thickness is 250 nm to obtain a CsI film. Then, a perovskite precursor 2 is deposited on the surface of the CsI film by atomic deposition technology. The perovskite precursor 2 includes lead(II)bis(trimethylsilyl)amide] (Pb(btsa)2) and tin(IV) iodide (SnI4). The deposition temperature is 100°C and the deposition thickness is 250 nm to obtain a CsPbI3 perovskite light absorbing layer with a thickness of 500 nm.
[0058] (5) BCPM and C are sequentially deposited on the surface of the CsPbI3 perovskite light-absorbing layer obtained in step (4). 60 The deposition rate was 0.02 nm / s. The film was then annealed at 100 °C for 10 min in a glove box to obtain an interface passivation layer with a thickness of 3 nm and a C layer with a thickness of 20 nm. 60 Electron transport layer.
[0059] (6) Using atomic deposition technology, the C 60 A layer of tin dioxide with a thickness of 15 nm is deposited on the surface of the electron transport layer to obtain a tin dioxide electron transport layer.
[0060] (7) A layer of silver metal electrode with a thickness of 120 nm is evaporated on the surface of the tin dioxide electron transport layer obtained in step (6), thereby obtaining the perovskite solar cell.
[0061] During the preparation process, C 60 The molecules will undergo a [2+2] cycloaddition reaction, C 60 A [4+2] cycloaddition reaction will occur between the C 60 Intermolecular [2+2] cycloaddition reaction and interfacial passivation agent and C 60 The schematic diagram of the [4+2] cycloaddition reaction between molecular layers is shown in Figure 1 shown.
[0062] In the perovskite cell, the interface passivation layer can be connected to C 60 Molecular layer assembly is achieved between the electron transport layer and the perovskite light absorbing layer, wherein the perovskite light absorbing layer 3, the interface passivation layer 2 and the C 60 The bonding structure diagram of the electron transport layer 1 is shown in Figure 2 shown.
[0063] Example 2
[0064] This embodiment provides a perovskite solar cell, which is different from the embodiment 1 only in that the thickness of the interface passivation layer is 5 nm, and other materials, structures and preparation methods are the same as those in the embodiment 1.
[0065] Example 3
[0066] This embodiment provides a perovskite solar cell, which is different from the embodiment 1 only in that the thickness of the interface passivation layer is 8 nm, and other materials, structures and preparation methods are the same as those in the embodiment 1.
[0067] Example 4
[0068] This embodiment provides a perovskite solar cell, which differs from the embodiment 1 only in that the annealing time in step (5) is 5 min, and the other materials, structures and preparation methods are the same as those in the embodiment 1.
[0069] Example 5
[0070] This embodiment provides a perovskite solar cell, which differs from the embodiment 1 only in that the annealing time in step (5) is 15 min, and the other materials, structures and preparation methods are the same as those in the embodiment 1.
[0071] Example 6
[0072] This embodiment provides a perovskite solar cell, which differs from the embodiment 1 only in that the annealing time in step (5) is 30 min, and the other materials, structures and preparation methods are the same as those in the embodiment 1.
[0073] Example 7
[0074] This embodiment provides a perovskite solar cell, which differs from the embodiment 1 only in that the annealing time in step (5) is 3 min, and the other materials, structures and preparation methods are the same as those in the embodiment 1.
[0075] Example 8
[0076] This embodiment provides a perovskite crystalline silicon stacked cell, and its structural schematic diagram is as follows Figure 4 As shown, the back conductive metal electrode 100, the back transparent conductive layer 101, the p-type amorphous silicon layer 102, the first intrinsic amorphous silicon layer 103, the silicon wafer 104, the second intrinsic amorphous silicon layer 105, the n-type amorphous silicon layer 106, the composite layer 107, the nickel oxide hole transport layer 108, the MeO-2PACz hole transport layer 109, the perovskite light absorption layer 110, the interface passivation layer 111, and the C 60 The electron transport layer 112, the tin dioxide electron transport layer 113, the front transparent conductive layer 114 and the front conductive metal electrode 115; the preparation method of the perovskite crystalline silicon stacked cell comprises the following steps:
[0077] (1) A semi-finished heterojunction cell is used as a crystalline silicon cell substrate, wherein the crystalline silicon cell substrate comprises a back conductive metal electrode 100, a back transparent conductive layer 101, a p-type amorphous silicon layer 102, a first intrinsic amorphous silicon layer 103, a silicon wafer 104, a second intrinsic amorphous silicon layer 105, and an n-type amorphous silicon layer 106 stacked in sequence; and a 30 nm thick ITO composite layer is sputtered on the surface of the n-type amorphous silicon layer by physical vapor deposition (PVD);
[0078] (2) A layer of nickel oxide with a thickness of 15 nm is sputtered on the surface of the ITO composite layer obtained in step (1) by a magnetron sputtering method to obtain a nickel oxide hole transport layer.
[0079] (3) Spin-coat the surface of the nickel oxide hole transport layer obtained in step (2) with a MeO-2PACz solution (the solvent is methanol and the concentration is 1 mM) at a spin-coating speed of 3000 rad / s; then anneal at 100°C for 10 min to obtain a MeO-2PACz hole transport layer with a thickness of 5 nm.
[0080] (4) preparing a perovskite precursor solution: including 1.05 mol / L PbI2, 0.35 mol / L PbBr2, 0.03 mol / L CsI, 1.05 mol / L FAI and 0.35 mol / L MABr, adding fluororana to make its concentration 0.02 M, and the solvent is a mixed solution of DMF and DMSO in a volume ratio of 4:1; then coating the surface of the hole transport layer obtained in step (3) with the perovskite precursor solution, spin coating at 1000 rpm for 10 s, and then spin coating at 5000 rpm for 30 s, at the initial moment of rotation at 5000 rpm, adding 140 μL of ethyl acetate to the sample surface, and obtaining a perovskite liquid film after the rotation ends; annealing the perovskite liquid film at 110°C for 10 min to obtain a perovskite light absorbing layer of about 500 nm thick.
[0081] (5) BCPM and C are sequentially deposited on the surface of the perovskite light-absorbing layer obtained in step (4).60 The deposition rate was 0.02 nm / s. The film was then annealed at 100 °C for 10 min in a glove box to obtain an interface passivation layer with a thickness of 5 nm and a C layer with a thickness of 20 nm. 60 Electron transport layer.
[0082] (6) Using atomic deposition technology, the C 60 A layer of tin dioxide with a thickness of 15 nm is deposited on the surface of the electron transport layer to obtain a tin dioxide electron transport layer.
[0083] (7) A layer of ITO film is sputtered on the surface of the tin dioxide electron transport layer obtained in step (6) to obtain a front transparent conductive layer with a thickness of 120 nm.
[0084] (8) A layer of silver metal electrode with a thickness of 900 nm is evaporated on the surface of the front transparent conductive layer obtained in step (7), thereby obtaining the perovskite crystalline silicon stacked cell.
[0085] Comparative Example 1
[0086] This comparative example provides a perovskite solar cell, which differs from Example 1 only in that there is no interface passivation layer. The preparation method comprises: obtaining a perovskite light absorbing layer in step (4) by evaporating C 60 , and a C layer with a thickness of 20 nm is obtained. 60 The electron transport layer, other materials, structures and preparation methods are the same as those in Example 1.
[0087] Comparative Example 2
[0088] This comparative example provides a perovskite crystalline silicon tandem cell, which differs from Example 7 only in that there is no interface passivation layer. The preparation method comprises: obtaining a perovskite light absorbing layer in step (4) by evaporating C 60 , and a C layer with a thickness of 20 nm is obtained. 60 The electron transport layer, other materials, structures and preparation methods are the same as those in Example 7.
[0089] Comparative Example 3
[0090] This comparative example provides a perovskite solar cell, which is different from Example 1 only in that the interface passivation layer and C 60 There is no cycloaddition reaction between the electron transport layers. In the preparation method, step (5) comprises: after evaporating BCPM on the surface of the CsPbI3 perovskite light absorbing layer obtained in step (4), annealing at 100°C for 10 min, and then evaporating C on the surface of the obtained interface passivation layer. 60 The electron transport layer is then directly processed into step (6). Other materials, structures and preparation methods are the same as those in Example 1.
[0091] Comparative Example 4
[0092] This comparative example provides a perovskite solar cell, which differs from Example 1 only in that BCPM is replaced by an equal amount of maleimidohexanoylhydrazide mono(trifluoroacetic acid) salt, and other materials, structures and preparation methods are the same as those in Example 1.
[0093] Performance Testing
[0094] The open circuit voltage (Voc), short circuit current (Jsc), fill factor (FF) and initial photoelectric conversion efficiency (PCE) of the perovskite cells provided in Examples 1 to 8 and Comparative Examples 1 to 4 were tested; the test results are shown in Table 1.
[0095] In addition, taking Example 2 and Comparative Example 1 as examples, the changes in the conversion efficiency of the perovskite battery over time were tested. The results are as follows: Figure 5 As shown, it can be seen that the conversion efficiency of the perovskite battery provided by the present invention decreases slightly with the extension of the use time, and the conversion efficiency can still reach more than 90% of the initial conversion efficiency after 1400 hours; while the comparative example 1 can only reach about 75% of the initial conversion efficiency, which proves that the perovskite battery provided by the present invention has better stability and longer service life.
[0096] Table 1
[0097]
[0098] As shown in Table 1, the perovskite cell provided by the present invention has improved the open circuit voltage, short circuit current and fill factor of the single junction perovskite solar cell and the perovskite crystalline silicon stacked cell by setting a specific interface passivation layer between the perovskite light absorption layer and the electron transport layer, and the conversion efficiency is also improved. This is because the interface passivator can be anchored on the perovskite surface to passivate the surface defects of the perovskite, and can also react with C 60 Achieve molecular layer assembly and lock C 60 , making it not easy to fall off, quickly transmitting carriers, enhancing the service life of the perovskite battery and improving device performance.
[0099] In the present invention, the conversion efficiency of the single-junction perovskite solar cell including the interface passivation layer reaches 19.23-20.39%, and after 1400 hours of use, the conversion efficiency can still reach more than 90% of the initial value, and the service life is long; while the conversion efficiency of the perovskite crystalline silicon solar cell reaches more than 30%; compared with the comparative example, the efficiency and service life of the perovskite cell provided by the present invention are greatly improved.
[0100] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A perovskite battery, characterized in that: An interface passivation layer is provided between the perovskite light absorption layer and the electron transport layer of the perovskite cell; The raw material of the interface passivation layer includes 3,5-di(carboxylic acid)-phenyl-3-maleimide; The electron transport layer includes fullerene and its derivative electron transport layer; The interface passivation layer and the perovskite light absorbing layer are connected via a surface synthesis reaction; The interface passivation layer and the electron transport layer are connected via a cycloaddition reaction; The general structural formula of the material of the perovskite light absorbing layer is ABX3; Wherein, A is selected from CH3NH3 + 、CH(NH2)2 + , Rb + or Cs + Any one or a combination of at least two of the following: B is selected from Pb 2+ ,Ge 2+ Sn 2+ Any one or a combination of at least two of; X is selected from Cl - Br - or I - Any one or a combination of at least two of the following.
2. The perovskite battery according to claim 1, characterized in that: The thickness of the interface passivation layer is 1-10 nm.
3. The perovskite battery according to claim 1, characterized in that: The thickness of the perovskite light-absorbing layer is 400-700 nm.
4. The perovskite battery according to claim 1, characterized in that: The thickness of the fullerene and its derivative electron transport layer is 10-30 nm; The side of the fullerene and its derivative electron transport layer away from the interface passivation layer is also provided with SnO x Electron transport layer; the SnO x The thickness of the electron transport layer is 5~20 nm.
5. The perovskite battery according to claim 1, characterized in that: A hole transport layer is also provided on the side of the perovskite light absorption layer away from the interface passivation layer; The material of the hole transport layer includes nickel oxide and / or [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid; The thickness of the hole transport layer is 10-20 nm.
6. The perovskite battery according to claim 5, characterized in that: The perovskite cell includes a single-junction perovskite solar cell and / or a perovskite crystalline silicon stacked cell; A conductive glass substrate is also provided on the side of the hole transport layer of the single-junction perovskite solar cell away from the perovskite light absorption layer; The conductive glass substrate includes any one of an indium tin oxide conductive glass substrate, a fluorine-doped SnO2 conductive glass substrate or an aluminum-doped ZnO conductive glass substrate; An electrode is also provided on the side of the electron transport layer of the single-junction perovskite solar cell away from the interface passivation layer; The electrode comprises a metal electrode; the thickness of the metal electrode is 80-150 nm.
7. The perovskite cell according to claim 6, characterized in that: The hole transport layer of the perovskite crystalline silicon stacked cell is also provided with a composite layer and a crystalline silicon cell substrate in sequence on the side away from the perovskite light absorption layer; The composite layer includes at least one of an indium tin oxide composite layer, a fluorine-doped SnO2 composite layer or an aluminum-doped ZnO composite layer; the thickness of the composite layer is 20-40 nm; An electrode is also provided on the side of the electron transport layer of the perovskite crystalline silicon stacked cell away from the interface passivation layer; the electrode comprises a metal electrode; and the thickness of the metal electrode is 800-1000 nm.
8. The perovskite cell according to claim 7, characterized in that: In the perovskite crystalline silicon stacked cell, a conductive layer is also provided between the electron transport layer and the electrode; The material of the conductive layer includes at least one of indium tin oxide, fluorine-doped SnO2 or aluminum-doped ZnO; the thickness of the conductive layer is 80-140 nm.
9. A method for preparing a perovskite battery according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: The raw materials of the interface passivation layer and fullerene and its derivatives are sequentially deposited on the surface of the perovskite light absorption layer, and annealed to obtain the interface passivation layer connected to the perovskite light absorption layer and the electron transport layer through chemical bonds.
10. The preparation method according to claim 9, characterized in that: The deposition method includes evaporation; the deposition rate is 0.01-0.05 nm / s; The annealing temperature is 80-120° C. and the annealing time is 3-15 min.