Anti-slip functional multi-layer carpet and its manufacturing process

By using a multi-layer structure of composite rubber layer and chemical fiber layer in the carpet, combined with acrylic fabric and waterproof ink, the problem of insufficient wear resistance and heat and oxygen aging resistance of TPR materials is solved, and the wear resistance and high temperature resistance of the carpet are significantly improved. and antioxidant properties, extending service life and improving carpet comfort and slip resistance.

CN118478537BActive Publication Date: 2024-10-22深せん市怡怡信息科技有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410284500.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-10-22
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

The TPR material of existing carpets has poor wear resistance and thermal oxygen aging resistance, resulting in a short service life.

Method used

Using a production process of anti-slip functional multi-layer carpet, by combining rubber material with mesh cotton cloth and non-woven fabric, and adding compound wear-resistant modifiers and high-temperature oxidation resistance additives to the rubber material, through a special process Let it penetrate and form to form a composite rubber layer and chemical fiber layer, combined with acrylic fabric and waterproof ink to form a multi-layer structure.

Benefits of technology

It significantly improves the wear resistance, high temperature resistance and oxidation resistance of the carpet, extends the service life of the carpet, and at the same time solves the problems of difficult care, high maintenance costs and insufficient anti-slip of traditional carpets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118478537B_ABST
    Figure CN118478537B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of carpets, and discloses a non-slip functional multi-layer carpet and a manufacturing process thereof. The multi-layer carpet comprises an ink layer, a chemical fiber layer, a non-woven fabric layer and a composite rubber layer from top to bottom. By effectively combining different materials, the carpet can have the advantages of being easy to care for, foldable, easy to clean and the like. The composite rubber layer is a flexible composite material formed by mutually fusing and interweaving a rubber material and a mesh cotton cloth, and can show good non-slip properties. The rubber material is prepared by extrusion granulation of SBS, polystyrene, epoxy natural rubber, a composite wear-resistant modifier, a high-temperature oxidation resistant additive, benzoyl peroxide and white oil. By adding the composite wear-resistant modifier and the high-temperature oxidation resistant additive, the rubber material can have the properties of abrasion resistance, high-temperature resistance and oxidation resistance, thereby extending the service life of the carpet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carpets, and in particular to an anti-slip functional multi-layer carpet and a manufacturing process thereof. Background Art

[0002] In modern society, carpets have become an important part of home decoration. Whether it is the living room, bedroom or corridor, you can see carpets. It not only beautifies the living environment, but also improves the comfort of the living environment. At the same time, carpets are also an environmentally friendly household item. They can also reduce noise and maintain indoor temperature, so they are deeply loved by consumers.

[0003] At present, carpets are mainly divided into pure wool carpets, chemical fiber carpets and plastic carpets. Pure wool carpets are mainly made of natural fibers such as wool. Although they are more comfortable, they are difficult to clean, are not corrosion-resistant, and are prone to mildew. Although chemical fiber carpets can overcome the shortcomings of pure wool carpets, they have poor anti-slip properties and pose a safety hazard. Although plastic carpets have good anti-slip effects, plastic is less comfortable, difficult to fold, and has poor wear resistance. Therefore, the carpets currently produced on the market have more or less certain defects.

[0004] In order to solve the defects of existing carpets, chemical fiber carpets and plastic carpets are combined to form a multi-layer structure carpet, which can take advantage of the advantages of both materials and make the carpet have good comfort and anti-slip properties. Acrylic fiber is commonly known as "artificial wool" and has a high degree of comfort. It can be used as the chemical fiber layer material of the carpet. TPR is a thermoplastic rubber material with excellent anti-slip and shock absorption properties. It uses SBS as the basic raw material and is matched with polystyrene resin, plasticizer and other additives. It can be processed and formed without vulcanization, so it can be used to make the plastic layer of multi-layer carpets. However, the wear resistance of TPR material itself is poor. Long-term friction with the ground may cause slag and other phenomena. At the same time, its antioxidant performance is poor. Especially in the north where heating is supplied, the carpet is in contact with the high temperature ground environment for a long time, which will accelerate the aging of the carpet and greatly shorten the service life of the carpet. Therefore, it is of great significance to produce TPR materials with excellent wear resistance and heat-oxidation aging resistance for the further development of carpets. Summary of the invention

[0005] The purpose of the present invention is to provide a non-slip functional multi-layer carpet and a manufacturing process thereof, which solves the problem that the TPR material has poor wear resistance and thermal oxygen aging resistance, resulting in a short service life of the carpet.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A production process of a non-slip functional multi-layer carpet comprises the following steps:

[0008] The first step is to place the rubber material in a temperature environment of 160-180°C to melt it to form a molten rubber material, pour the molten rubber material into a mold equipped with a mesh cotton cloth, and make it completely penetrate into the mesh cotton cloth, and then extrude it into shape through an extrusion process, let it stand, and cool it naturally to form a composite rubber layer;

[0009] The second step is to cover the non-woven fabric on the surface of the uncooled composite rubber layer, and use pressurization and heat fusion to make the composite rubber layer fully penetrate into the non-woven fabric layer. After cooling, the non-woven fabric can be attached to the upper surface of the composite rubber layer to form a non-woven fabric layer;

[0010] Step 3: Use a 360° rotating roller to evenly coat the polyacrylate pressure-sensitive adhesive on the upper surface of the non-woven fabric layer, and control the coating amount to 240-250g / m 2 After coating, the acrylic fabric is covered on the upper side of the non-woven fabric layer, extruded and formed by the extrusion process, and then left to stand for 30-40 minutes to form a chemical fiber layer;

[0011] Step 4: Turn on the heat transfer machine, set the temperature to 120-140℃, transfer the waterproof ink to the surface of the chemical fiber layer to form a waterproof ink layer, and then go through trimming and shearing processes to obtain a multi-layer carpet.

[0012] In the first step, the rubber material includes the following raw materials in parts by weight: 65-75 parts of SBS, 15-25 parts of polystyrene, 10-20 parts of epoxy natural rubber, 3-5 parts of composite wear-resistant modifier, 4-6 parts of high temperature oxidation resistance additive, 0.1-0.5 parts of benzoyl peroxide, and 40-55 parts of white oil.

[0013] Specifically, the rubber material is first melted at high temperature into a flowable liquid material so that it can completely fill each small hole in the mesh cotton cloth and be densely distributed on both sides of the mesh cotton cloth. Then, through an extrusion molding process, the rubber material can completely penetrate into the mesh cotton cloth. After the rubber liquid material is cooled, it can form a flexible composite material that is fused and interwoven with the mesh cotton cloth. This flexible composite material not only has good anti-slip properties, but can also be folded and can be directly machine washed, and has strong plasticity.

[0014] Further preferably, the epoxidation degree of the epoxidized natural rubber is 25%.

[0015] Further preferably, the preparation method of the composite wear-resistant modifier comprises the following steps:

[0016] Step A: Prepare mixed dispersion

[0017] The basalt fiber and purified water are mixed and ultrasonically dispersed to form a fiber dispersion with a mass fraction of 5%; the zinc oxide whisker and purified water are mixed and ultrasonically dispersed to form a zinc oxide dispersion with a mass fraction of 2%; the fiber dispersion and the zinc oxide dispersion are mixed to form a mixed dispersion;

[0018] Step B: Preparation of composite wear-resistant modifier

[0019] Under continuous stirring, add bis(3-(triethoxysilyl)propylamine) to the mixed dispersion. After the addition, use acetic acid to adjust the pH to 3-4, heat and control the temperature to maintain the temperature at 70-80°C. After stirring for 3-6 hours, separate and collect the solid material to obtain a composite wear-resistant modifier.

[0020] Specifically, the siloxane groups in the structure of bis (3-(triethoxysilyl)propylamine can be hydrolyzed under acidic conditions to produce highly active silanol groups, which condense with the hydroxyl groups on the surfaces of basalt fibers and zinc oxide whiskers, thereby achieving an organic combination of zinc oxide whiskers and basalt fibers with bis (3-(triethoxysilyl)propylamine as a bridging agent to produce a composite wear-resistant modifier.

[0021] Further preferably, in step A, the diameter of the basalt fiber is 10-20 μm and the length is 1-2 mm; the average particle size of the zinc oxide whisker is 100 nm.

[0022] Further preferably, in step A, the volume ratio of the fiber dispersion to the zinc oxide dispersion in the mixed dispersion is 1:1.

[0023] Further preferably, the preparation method of the anti-high temperature oxidation aid comprises the following steps:

[0024] Step S1: preparing modified polysiloxane

[0025] 3-glycidyloxypropyl-terminated dimethyl polysiloxane and toluene are mixed evenly to form a homogeneous liquid material, N-hydroxy-5-norbornene-2,3-dicarboximide and boron trifluoride ether complex are added to the liquid material, and after the addition, the temperature is raised until the temperature reaches 60-70° C., and after stirring for 4-6 hours at this temperature, the solvent is evaporated to obtain a modified polysiloxane;

[0026] Specifically, 3-glycidyloxypropyl terminated dimethyl polysiloxane contains a terminal epoxy group, which can undergo ring-opening with the hydroxyl group of N-hydroxy-5-norbornene-2,3-dicarboximide under the catalytic action of boron trifluoride ether complex, thereby achieving the organic combination of norbornene heterocycle and rigid imide heterocycle with polysiloxane to obtain modified polysiloxane.

[0027] Step S2: preparing high temperature oxidation resistance additive

[0028] Add gallic acid to tetrahydrofuran, stir and mix evenly, then add condensing agent and dehydrating agent, stir and mix for 20-30 minutes, then continue to add modified polysiloxane, mix evenly after adding, mechanically stir for 6-9 hours at room temperature, evaporate and remove the solvent, and the obtained is the anti-high temperature oxidation additive.

[0029] Gallic acid is activated by using a condensation agent and a dehydrating agent so that it can undergo dehydration condensation with the active hydroxyl groups generated by the ring-opening reaction in the modified polysiloxane structure, thereby further introducing the natural antioxidant gallic acid into the polysiloxane structure to prepare an anti-high temperature oxidation additive.

[0030] Further preferably, in step S1, the weight average molecular weight of the 3-glycidyloxypropyl terminated dimethylpolysiloxane is 3000.

[0031] Further preferably, in step S2, the condensing agent is dicyclohexylcarbodiimide or 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride; and the dehydrating agent is at least one of N-hydroxysuccinimide, 4-dimethylaminopyridine or 1-hydroxybenzotriazole.

[0032] Further preferably, the method for preparing the rubber material comprises the following steps:

[0033] SBS, polystyrene, epoxy natural rubber, composite wear-resistant modifier, high-temperature oxidation resistance aid, benzoyl peroxide and white oil are added to an internal mixer in sequence, and the internal mixing temperature is controlled to be 130-150°C. After internal mixing for 5-10 minutes, the materials are transferred to an extruder, and the screw aspect ratio is set to 45-55:1 and the screw speed is set to 200-300rpm. The rubber material can be obtained by extrusion granulation at a temperature of 160-170°C.

[0034] Specifically, since the high temperature oxidation resistance agent contains norbornene groups in its structure, it can undergo melt polymerization with the SBS matrix under the action of benzoyl peroxide in a high temperature molten state, thereby combining the high temperature oxidation resistance agent with the SBS matrix.

[0035] A non-slip functional multi-layer carpet is prepared by adopting the preparation method.

[0036] Beneficial effects of the present invention:

[0037] (a) The present invention uses bis(3-(triethoxysilyl)propylamine) as a bridging agent to organically combine basalt fiber and zinc oxide whisker to obtain a composite wear-resistant modifier. On the one hand, zinc oxide whisker can slide relatively on the surface of basalt fiber, producing a unique "ball effect", thereby achieving a good wear reduction effect, so that the obtained rubber material can exhibit good wear resistance. On the other hand, the bridging agent contains active secondary amino groups, which can interact with the raw material epoxidized natural rubber in the rubber material during the high-temperature melting process, thereby generating a higher bonding force between the composite wear-resistant modifier and the rubber matrix, thereby effectively exerting the role of basalt fiber and making the rubber material exhibit more excellent mechanical properties.

[0038] (b) The high-temperature oxidation resistance additive prepared by the present invention contains a large number of silicon-oxygen bonds in its structure, as well as rigid imide and norbornene heterocycles. The presence of these structures will require the rubber to absorb more heat when decomposing, so that the prepared rubber material can exhibit excellent high-temperature resistance. At the same time, the natural antioxidant gallic acid contained in the high-temperature oxidation resistance additive structure can effectively enhance the aging resistance of the rubber, so that the prepared rubber material exhibits good antioxidant properties. In addition, since the high-temperature oxidation resistance additive will combine with the rubber molecular chain during the high-temperature melting process, the gallic acid can be stably present in the rubber material, so that the rubber material has a longer aging resistance period, thereby making the carpet have a longer service life.

[0039] (c) The present invention adopts a special manufacturing process to effectively combine different materials and effectively utilize the advantages and characteristics of various materials, thereby solving the shortcomings of traditional carpets such as difficult care, high maintenance cost, inability to fold, and high difficulty in cleaning.

[0040] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0042] Figure 1 This is an infrared image of the anti-high temperature oxidation additive in Example 2 of the present invention. DETAILED DESCRIPTION

[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] Example 1

[0045] Preparation of composite wear-resistant modifier

[0046] Step A: Prepare mixed dispersion

[0047] Basalt fibers with a diameter of 15 μm and a length of 1 mm were mixed with purified water, and ultrasonically dispersed to form a fiber dispersion with a mass fraction of 5%; zinc oxide whiskers with an average particle size of 100 nm were mixed with purified water, and ultrasonically dispersed to form a zinc oxide dispersion with a mass fraction of 2%; 100 mL of the fiber dispersion and 100 mL of the zinc oxide dispersion were mixed to form a mixed dispersion;

[0048] Step B: Preparation of composite wear-resistant modifier

[0049] Under constant stirring, add 2.6 g of bis(3-(triethoxysilyl)propyl)amine to 200 mL of the mixed dispersion. After the addition, adjust the pH to 3 with acetic acid, heat and control the temperature to maintain it at 75°C. After stirring for 4 hours, separate and collect the solid material to obtain a composite wear-resistant modifier.

[0050] Example 2

[0051] Preparation of high temperature oxidation resistance additive

[0052] Step S1: preparing modified polysiloxane

[0053] 3.5 g of 3-glycidyloxypropyl-terminated dimethyl polysiloxane having a weight average molecular weight of 3000 was uniformly mixed with toluene to form a homogeneous liquid material, 0.42 g of N-hydroxy-5-norbornene-2,3-dicarboximide and 0.2 g of boron trifluoride ether complex were added to the liquid material, and after the addition, the temperature was raised until the temperature reached 65° C., and after stirring for 6 hours at this temperature, the solvent was evaporated to obtain a modified polysiloxane;

[0054] Step S2: preparing high temperature oxidation resistance additive

[0055] Add 0.3 g of gallic acid to tetrahydrofuran, stir and mix evenly, then add 0.1 g of dicyclohexylcarbodiimide and 0.03 g of 4-dimethylaminopyridine, stir and mix for 30 minutes, then continue to add 2.8 g of modified polysiloxane, mix well after adding, mechanically stir at room temperature for 8 hours, evaporate and remove the solvent, and the result is an anti-high temperature oxidation additive.

[0056] The infrared test of the anti-high temperature oxidation additive was carried out using Nicolet 6700 Fourier transform infrared spectrometer, with a spectral range of 4000-500cm -1 The analysis results are shown in Figure 1 , of which 3391cm -1 The absorption peak at 3034 cm is attributed to the -OH stretching vibration peak in gallic acid. -1 The absorption peak at 2945-1875cm is attributed to the carbon-hydrogen stretching vibration absorption peak of the C=C double bond in norbornene. -1 The absorption peak at 1748 cm is attributed to the carbon-hydrogen stretching vibration absorption peak of methyl, ethyl and methine. -1 The absorption peak at 1666cm is attributed to the C=O stretching vibration absorption peak generated by the condensation reaction. -1 The absorption peak at 1117 cm is attributed to the C=O stretching vibration absorption peak in the imide. -1 The absorption peak at 1062 cm is attributed to the ether bond stretching vibration absorption peak generated by the ring-opening reaction. -1 The absorption peak that appears at is attributed to the Si-O stretching vibration absorption peak in polysiloxane.

[0057] Example 3

[0058] The preparation method of the rubber material is specifically as follows:

[0059] 65 parts of SBS, 15 parts of polystyrene, 10 parts of epoxy natural rubber with an epoxidation degree of 25%, 3 parts of the composite wear-resistant modifier prepared in Example 1 of the present invention, 4 parts of the high-temperature oxidation resistant additive prepared in Example 2 of the present invention, 0.1 parts of benzoyl peroxide and 40 parts of white oil were added to an internal mixer in sequence, and the internal mixing temperature was controlled to be 130° C. After internal mixing for 5 minutes, the material was transferred to an extruder, the screw aspect ratio was set to 50:1, the screw speed was set to 200 rpm, and extrusion granulation was performed at a temperature of 160° C. to obtain a rubber material.

[0060] Example 4

[0061] The preparation method of the rubber material is specifically as follows:

[0062] 70 parts of SBS, 18 parts of polystyrene, 16 parts of epoxy natural rubber with an epoxidation degree of 25%, 4.5 parts of the composite wear-resistant modifier prepared in Example 1 of the present invention, 5 parts of the high-temperature oxidation resistant additive prepared in Example 2 of the present invention, 0.4 parts of benzoyl peroxide and 50 parts of white oil were added to an internal mixer in sequence, and the internal mixing temperature was controlled to be 140° C. After internal mixing for 10 minutes, the material was transferred to an extruder, the screw aspect ratio was set to 50:1, the screw speed was set to 300 rpm, and extrusion granulation was performed at a temperature of 170° C. to obtain a rubber material.

[0063] Example 5

[0064] The preparation method of the rubber material is specifically as follows:

[0065] 75 parts of SBS, 25 parts of polystyrene, 20 parts of epoxy natural rubber with an epoxidation degree of 25%, 5 parts of the composite wear-resistant modifier prepared in Example 1 of the present invention, 6 parts of the high-temperature oxidation resistant additive prepared in Example 2 of the present invention, 0.5 parts of benzoyl peroxide and 55 parts of white oil were added to an internal mixer in sequence, and the internal mixing temperature was controlled to be 150° C. After internal mixing for 10 minutes, the material was transferred to an extruder, the screw aspect ratio was set to 50:1, the screw speed was set to 300 rpm, and extrusion granulation was performed at a temperature of 170° C. to obtain a rubber material.

[0066] Comparative Example 1

[0067] The preparation method of the rubber material is specifically as follows:

[0068] 70 parts of SBS, 18 parts of polystyrene, 16 parts of epoxy natural rubber with an epoxidation degree of 25%, 4.5 parts of basalt fiber, 5 parts of the high-temperature oxidation resistance additive prepared in Example 2 of the present invention, 0.4 parts of benzoyl peroxide and 50 parts of white oil were added to an internal mixer in sequence, and the internal mixing temperature was controlled to be 140°C. After internal mixing for 10 minutes, the materials were transferred to an extruder, and the screw aspect ratio was set to 50:1 and the screw speed was set to 300 rpm. The rubber material was extruded and granulated at a temperature of 170°C to obtain the rubber material.

[0069] Comparative Example 2

[0070] The preparation method of the rubber material is specifically as follows:

[0071] 70 parts of SBS, 18 parts of polystyrene, 16 parts of epoxy natural rubber with an epoxidation degree of 25%, 5 parts of the high temperature oxidation resistance aid prepared in Example 2 of the present invention, 0.4 parts of benzoyl peroxide and 50 parts of white oil were added to an internal mixer in sequence, and the internal mixing temperature was controlled to be 140°C. After internal mixing for 10 minutes, the materials were transferred to an extruder, and the screw aspect ratio was set to 50:1 and the screw speed was set to 300 rpm. The rubber material was extruded and granulated at a temperature of 170°C to obtain the rubber material.

[0072] Comparative Example 3

[0073] The preparation method of the rubber material comprises the following steps:

[0074] 70 parts of SBS, 18 parts of polystyrene, 16 parts of epoxy natural rubber with an epoxidation degree of 25%, 4.5 parts of the composite wear-resistant modifier prepared in Example 1 of the present invention, 0.4 parts of benzoyl peroxide and 50 parts of white oil were added to an internal mixer in sequence, and the internal mixing temperature was controlled to be 140° C. After internal mixing for 10 minutes, the materials were transferred to an extruder, the screw aspect ratio was set to 50:1, the screw speed was set to 300 rpm, and extrusion granulation was performed at a temperature of 170° C. to obtain a rubber material.

[0075] Comparative Example 4

[0076] The preparation method of the rubber material is specifically as follows:

[0077] 70 parts of SBS, 18 parts of polystyrene, 16 parts of epoxy natural rubber with an epoxidation degree of 25%, 0.4 parts of benzoyl peroxide and 50 parts of white oil are added into an internal mixer in sequence, and the internal mixing temperature is controlled to be 140°C. After internal mixing for 10 minutes, the materials are transferred to an extruder, and the screw aspect ratio is set to 50:1 and the screw speed is set to 300 rpm. The rubber material can be obtained by extrusion granulation at a temperature of 170°C.

[0078] The rubber materials prepared in Examples 3 to 5 and Comparative Examples 1 to 4 were tested for performance, and the results are shown in the following table:

[0079] ,

[0080] Note: The tensile properties are tested according to GB / T 528-2009. After the test, the test samples of the same specifications are placed in an aging box at 80°C for accelerated aging for 24 hours, and then the tensile properties are tested again; the wear resistance is tested according to GB / T 1689-2014; the test method for the initial decomposition temperature is: weigh each group of samples of the same mass, place them in a thermogravimetric analyzer, control the heating rate to 5°C / min, increase the temperature from room temperature to 600°C, and record the temperature when the sample loses 5% of its weight, which is the initial decomposition temperature.

[0081] From the test results in the analysis table, it can be seen that compared with the comparative example 4 in which the composite wear-resistant modifier and the high-temperature oxidation resistance additive were not added, the rubber materials prepared in Examples 3 to 5 obviously have good mechanical strength, wear resistance and high-temperature oxidation resistance. Comparative example 1 uses a single basalt fiber as a filler, which obviously loses the "ball effect", resulting in a significant decline in wear resistance. Comparative example 2 does not add basalt fiber, and not only has poor wear resistance, but also a significant decrease in mechanical strength. The rubber material prepared in Comparative example 3 does not add an anti-high-temperature oxidation additive, and the high-temperature resistance and aging resistance performance decline significantly.

[0082] The rubber material prepared in Example 4 of the present invention is used to prepare a multi-layer carpet, and the manufacturing process includes the following steps:

[0083] The first step is to place the rubber material in a temperature environment of 180°C to melt it to form a molten rubber material, pour the molten rubber material into a mold equipped with a mesh cotton cloth, and make it completely penetrate into the mesh cotton cloth, and then extrude it into shape through an extrusion process, let it stand, and cool it naturally to form a composite rubber layer;

[0084] The second step is to cover the non-woven fabric on the surface of the uncooled composite rubber layer, and use the method of pressurization and heat fusion, setting the pressure to 2MPa and the fusion temperature to 200℃, so that the composite rubber layer can fully penetrate into the non-woven fabric layer. After cooling, the non-woven fabric can be attached to the upper surface of the composite rubber layer to form a non-woven fabric layer;

[0085] Step 3: Use a 360° rotating roller to evenly coat the polyacrylate pressure-sensitive adhesive on the upper surface of the non-woven fabric layer, and control the coating amount to 240g / m 2 After coating, the acrylic fabric is covered on the upper side of the non-woven fabric layer, extruded and formed by the extrusion process, and then left to stand for 30 minutes to form a chemical fiber layer;

[0086] Step 4: Turn on the heat transfer machine, set the temperature to 130°C, transfer the TPU waterproof ink to the surface of the chemical fiber layer to form a waterproof ink layer, and then go through trimming and shearing processes to obtain a multi-layer carpet.

[0087] The present invention arranges a waterproof ink layer on the upper surface of the carpet, so that the carpet has a good dirt resistance effect, and through the heat transfer process, different patterns and designs can be designed to avoid the deficiency of the carpet visual effect monomer, and at the same time, a chemical fiber layer is arranged to make the carpet softer and more comfortable, and a composite rubber layer containing mesh cotton cloth and rubber material is arranged on the bottom. Under the action of the mesh cotton cloth, the composite rubber layer can form a special mesh structure, and this mesh structure can make the carpet have a good anti-slip effect, avoiding the deficiency of the traditional carpet that needs to add an anti-slip pad. In addition, the raw material of the rubber material is uniquely designed, so that the prepared carpet has more excellent wear resistance and high temperature oxidation resistance, which is beneficial to prolonging the service life of the carpet.

[0088] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A process for producing a non-slip functional multi-layer carpet, characterized in that: The following steps are involved: The first step is to place the rubber material in a temperature environment of 160-180°C to melt it to form a molten rubber material, pour the molten rubber material into a mold equipped with a mesh cotton cloth, make it completely penetrate into the mesh cotton cloth, and then extrude it into shape through an extrusion process to form a composite rubber layer; The second step is to cover the non-woven fabric on the surface of the uncooled composite rubber layer, and use pressurization and heat fusion to make the composite rubber layer fully penetrate into the non-woven fabric layer. After cooling, the non-woven fabric can be attached to the upper surface of the composite rubber layer to form a non-woven fabric layer; Step 3: Use a 360° rotating roller to evenly coat the polyacrylate pressure-sensitive adhesive on the upper surface of the non-woven fabric layer, and control the coating amount to 240-250g / m 2 After coating, the acrylic fabric is covered on the upper side of the non-woven fabric layer, extruded and formed by the extrusion process, and then left to stand for 30-40 minutes to form a chemical fiber layer; Step 4: Turn on the heat transfer machine, set the temperature to 120-140℃, transfer the waterproof ink to the surface of the chemical fiber layer to form a waterproof ink layer, and then go through the trimming and shearing process to obtain a multi-layer carpet; In the first step, the rubber material includes the following raw materials in parts by weight: 65-75 parts of SBS, 15-25 parts of polystyrene, 10-20 parts of epoxy natural rubber, 3-5 parts of composite wear-resistant modifier, 4-6 parts of high temperature oxidation resistance additive, 0.1-0.5 parts of benzoyl peroxide, and 40-55 parts of white oil; The preparation method of the composite wear-resistant modifier comprises the following steps: Step A: Prepare mixed dispersion The basalt fiber and purified water are mixed and ultrasonically dispersed to form a fiber dispersion with a mass fraction of 5%; the zinc oxide whisker and purified water are mixed and ultrasonically dispersed to form a zinc oxide dispersion with a mass fraction of 2%; the fiber dispersion and the zinc oxide dispersion are mixed to form a mixed dispersion; Step B: Preparation of composite wear-resistant modifier Under continuous stirring, add bis(3-(triethoxysilyl)propylamine) to the mixed dispersion, adjust the pH to 3-4 with acetic acid, heat and control the temperature to maintain the temperature at 70-80°C, stir for 3-6h, separate and collect the solid material, and the obtained composite wear-resistant modifier is obtained; The preparation method of the high temperature oxidation resistance aid comprises the following steps: Step S1: preparing modified polysiloxane 3-glycidyloxypropyl-terminated dimethyl polysiloxane and toluene are mixed evenly to form a homogeneous liquid material, N-hydroxy-5-norbornene-2,3-dicarboximide and boron trifluoride ether complex are added to the liquid material, and after the addition is completed, the temperature is raised until the temperature reaches 60-70° C., stirred for 4-6 hours, and then the solvent is evaporated to obtain a modified polysiloxane; Step S2: preparing high temperature oxidation resistance additive Add gallic acid to tetrahydrofuran, stir and mix evenly, then add condensing agent and dehydrating agent, stir and mix for 20-30 minutes, then continue to add modified polysiloxane, mix evenly after adding, mechanically stir for 6-9 hours at room temperature, evaporate and remove the solvent, and the obtained is the anti-high temperature oxidation additive.

2. The manufacturing process of the anti-slip functional multi-layer carpet according to claim 1, characterized in that: The epoxidation degree of the epoxidized natural rubber is 25%.

3. The manufacturing process of the anti-slip functional multi-layer carpet according to claim 1, characterized in that: In step A, the diameter of the basalt fiber is 10-20 μm and the length is 1-2 mm; the average particle size of the zinc oxide whisker is 100 nm.

4. The manufacturing process of the anti-slip functional multi-layer carpet according to claim 1, characterized in that: In step A, the volume ratio of the fiber dispersion to the zinc oxide dispersion in the mixed dispersion is 1:

1.

5. The manufacturing process of the anti-slip functional multi-layer carpet according to claim 1, characterized in that: In step S1, the weight average molecular weight of the 3-glycidyloxypropyl terminated dimethylpolysiloxane is 3000.

6. The manufacturing process of the anti-slip functional multi-layer carpet according to claim 1, characterized in that: In step S2, the condensing agent is dicyclohexylcarbodiimide or 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride; and the dehydrating agent is at least one of N-hydroxysuccinimide, 4-dimethylaminopyridine or 1-hydroxybenzotriazole.

7. The manufacturing process of the anti-slip functional multi-layer carpet according to claim 1, characterized in that: The specific preparation method of the rubber material is as follows: SBS, polystyrene, epoxy natural rubber, composite wear-resistant modifier, high-temperature oxidation resistance aid, benzoyl peroxide and white oil are added to an internal mixer in sequence, and the internal mixing temperature is controlled to be 130-150°C. After internal mixing for 5-10 minutes, the materials are transferred to an extruder, and the screw aspect ratio is set to 45-55:1 and the screw speed is set to 200-300rpm. The rubber material can be obtained by extrusion granulation at a temperature of 160-170°C.

8. A non-slip functional multi-layer carpet, characterized in that: The method is prepared by the manufacturing process as claimed in claim 1.

Citation Information

Cited By

  • High-elasticity high-pressure impact-resistant wear-resistant rubber carpet and preparation process

    CN119684692A