A quaternary precursor material and preparation method thereof, and a preparation method of a positive electrode material
By preparing quaternary precursor materials and three-stage sintering processes, the electrochemical properties of sodium-ion battery cathode materials are improved, solving the shortcomings of existing materials in electrochemical performance and resource sustainability, and achieving higher cycle and rate performance and reduced production costs.
Patent Information
- Application Number
- CN202410939458.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Existing sodium-ion battery cathode materials have deficiencies in electrochemical performance and resource sustainability, especially nickel and manganese doped materials that cannot meet the needs of future power products.
The quaternary precursor material is prepared by the co-precipitation reaction of nickel, iron, manganese and copper, and the cathode material is prepared through a three-stage sintering process to improve the material's cycle performance and rate performance.
It effectively improves the electrochemical performance of the cathode material, achieves more uniform particle distribution and higher storage performance, reduces production costs, and has good application prospects.
Smart Images

Figure CN118479568B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of sodium ion battery materials and relates to a precursor material, in particular to a quaternary precursor material and a preparation method thereof, and a preparation method of a positive electrode material. Background Art
[0002] At present, there are three main types of cathodes: Prussian cathode, layered oxide cathode and polyanion cathode. Prussian cathode is a compound composed of sodium and ferrocyanide, usually blue, with the characteristics of high voltage and high energy density, simple preparation process and low cost; layered oxide cathode is composed of sodium and copper oxide, iron, manganese, nickel and other metals, with high energy density and long cycle life; polyanion cathode materials are sodium iron phosphate and sodium vanadium phosphate, etc., with high safety and long life.
[0003] The positive electrode materials of layered high energy density lithium-ion batteries use a large amount of cobalt, nickel and other materials, but the resources of cobalt and nickel are likely to be exhausted in the next 50 years. In contrast, layered sodium-ion battery positive electrode materials have more choices for 3d transition metals. Doping elements such as manganese and iron in the positive electrode materials can improve their electrochemical performance. Manganese and iron are both abundant elements in the earth's crust and have a wide range of material sources.
[0004] With the development of science and technology, positive electrode materials doped only with nickel and iron can no longer meet the battery needs of power products. Therefore, improving the electrochemical performance of positive electrode materials is an issue that technicians in this field urgently need to solve. Summary of the invention
[0005] In view of the above problems existing in the prior art, in the first aspect, the present invention provides a method for preparing a quaternary precursor material; in the second aspect, the present invention provides a quaternary precursor material; in the third aspect, the present invention provides a method for preparing a positive electrode material.
[0006] In a first aspect, a method for preparing a quaternary precursor material comprises the following steps:
[0007] Step 1, adding nickel salt, iron salt and manganese salt into water to obtain a mixed solution A;
[0008] Step 2: introducing sodium hydroxide solution, copper ammonia solution, mixed solution A and complexing agent into the bottom liquid of the reaction kettle, reacting for a period of time, filtering and drying to obtain a quaternary precursor material.
[0009] Preferably, the nickel salt is one or more of nickel sulfate, nickel chloride and nickel nitrate.
[0010] Preferably, the iron salt is one or more of ferrous sulfate, ferrous chloride and ferrous nitrate.
[0011] Preferably, the manganese salt is one or more of manganese sulfate, manganese chloride and manganese nitrate.
[0012] Preferably, the raw materials for preparing the copper ammonia solution include copper sulfate solution and ammonia water.
[0013] Preferably, the raw materials for preparing the reactor bottom liquid include sodium hydroxide solution and a complexing agent.
[0014] Preferably, in the mixed solution A and the cuprammonia solution, the molar ratio of nickel, iron, manganese and copper is 0.29-0.31:0.33-0.35:0.31-0.33:0.03-0.05, and the sum of the molar ratios of nickel, iron, manganese and copper is 1.
[0015] Preferably, the temperature of the reaction system is 50-70° C., the reaction time is 100-140 h; and the pH value of the reaction system is 10.2-11.1.
[0016] Preferably, the alkali solution is one or more of sodium hydroxide solution, potassium hydroxide solution and sodium bicarbonate solution; the concentration of the alkali solution is 8-10 mol / L.
[0017] Preferably, the complexing agent is one or more of ammonia water, oxalic acid and carbonate; the concentration of the complexing agent is 4-6 mol / L.
[0018] In a second aspect, a quaternary precursor material is prepared by the above-mentioned preparation method; the chemical formula of the quaternary precursor material is Ni x Fe y Mn z Cu u (OH)2, where 0.29≤x≤0.31, 0.33≤y≤0.35, 0.31≤z≤0.33, 0.03≤u≤0.05, and x+y+z+u=1.
[0019] Preferably, the quaternary precursor material is spherical in shape and has uniform particle distribution.
[0020] In a third aspect, a method for preparing a positive electrode material is provided, which comprises mixing the above-mentioned quaternary precursor material and a sodium source, and sintering the mixture in an oxygen atmosphere to obtain a nickel-iron-manganese-copper quaternary positive electrode material; wherein the sintering comprises three stages of sintering, and the sintering temperature of the three stages of sintering gradually increases.
[0021] Preferably, the sintering temperature of the first stage sintering is 300-500° C., and the sintering time is 60-120 min.
[0022] Preferably, the sintering temperature of the second stage sintering is 550-700° C., and the sintering time is 170-230 min.
[0023] Preferably, the sintering temperature of the third stage sintering is 700-950° C., and the sintering time is 15-20 hours.
[0024] Preferably, the sodium source is one or more of sodium carbonate, sodium bicarbonate and sodium oxalate.
[0025] Preferably, the mass ratio of the quaternary precursor material to the sodium source is 1:1.02-1.04.
[0026] Compared with the prior art, the present invention has the following obvious beneficial technical effects:
[0027] (1) In the process for preparing a quaternary precursor provided by the present invention, a quaternary precursor material is obtained by coprecipitation reaction of copper ammonia with a mixed solution of nickel, iron and manganese. The obtained quaternary precursor material has no agglomeration phenomenon and has a more uniform particle distribution; the synthesis of quaternary positive electrode materials can effectively improve the material's cycle performance, rate performance and storage performance.
[0028] (2) The method for preparing the precursor provided by the present invention is simple, low-cost, easy to implement, and has good application prospects.
[0029] (3) The three-stage sintering process is used to prepare positive electrode materials, which can improve the electrochemical properties of positive electrode materials and facilitate their promotion and commercialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a SEM image of the precursor material prepared in Example 1 of the present invention.
[0031] Figure 2 This is a SEM image of the precursor material prepared in Comparative Example 1 of the present invention.
[0032] Figure 3 This is a test chart of the cycle performance of batteries assembled with the positive electrode materials prepared in Examples 4 to 6 of the present invention and Comparative Examples 2 to 5.
[0033] Figure 4 This is a rate performance test diagram of batteries assembled with the positive electrode materials prepared in Examples 4 to 7 and Comparative Examples 2 to 5 of the present invention. DETAILED DESCRIPTION
[0034] The present invention provides the following specific technical solutions.
[0035] In a first aspect, a method for preparing a quaternary precursor material comprises the following steps:
[0036] Step 1, adding nickel salt, iron salt and manganese salt into water to obtain a mixed solution A;
[0037] Step 2: introducing sodium hydroxide solution, copper ammonia solution, mixed solution A and complexing agent into the bottom liquid of the reaction kettle, reacting for a period of time, filtering and drying to obtain a quaternary precursor material.
[0038] The inventors have found through research that when preparing precursor materials, the lattice oxygen ions are more stable after copper is doped, which effectively improves the electrochemical performance of the layered sodium ion positive electrode, further improves the interface stability of the material, and thus improves the electrochemical performance of the material.
[0039] The inventors further discovered that when preparing the precursor material, using a copper ammonia solution as the copper source, the obtained quaternary precursor material has low particle agglomeration and good dispersion.
[0040] Preferably, the nickel salt is one or more of nickel sulfate, nickel chloride and nickel nitrate.
[0041] Preferably, the iron salt is one or more of ferrous sulfate, ferrous chloride and ferrous nitrate.
[0042] Preferably, the manganese salt is one or more of manganese sulfate, manganese chloride and manganese nitrate.
[0043] Preferably, the raw materials for preparing the copper ammonia solution include copper sulfate solution and ammonia water.
[0044] In actual operation, other materials can be selected according to demand to prepare copper ammonia solution. In a specific embodiment of the present invention, copper sulfate and ammonia water are mixed to prepare copper ammonia, so as to avoid the introduction of impurity ions, improve the purity of the precursor material, avoid the interference of impurity ions, and thus improve the electrochemical performance of the positive electrode material.
[0045] Preferably, the raw materials for preparing the reactor bottom liquid include sodium hydroxide solution and a complexing agent.
[0046] Preferably, in the mixed solution A and the cuprammonia solution, the molar ratio of nickel, iron, manganese and copper is 0.29-0.31:0.33-0.35:0.31-0.33:0.03-0.05, and the sum of the molar ratios of nickel, iron, manganese and copper is 1.
[0047] In actual operation, the doping concentrations of nickel, iron, manganese and copper can be prepared according to actual needs.
[0048] Preferably, the temperature of the reaction system is 50-70° C., the reaction time is 100-140 h; and the pH value of the reaction system is 10.2-11.1.
[0049] In actual operation, the reaction temperature, reaction time and pH value can be selected according to the actual situation. The temperature of the reaction system is 50-70°C and the reaction time is 100-140h, which is the preferred range obtained by the inventors through multiple experiments. In a specific embodiment of the present invention, the temperature of the reaction system can be 50°C, 60°C, or 70°C; the reaction time can be 100h, 120h, or 140h; and the pH value of the reaction system can be 10.2, 10.7, or 11.1.
[0050] Preferably, the alkali solution is one or more of sodium hydroxide solution, potassium hydroxide, and sodium bicarbonate; and the concentration of the alkali solution is 8-10 mol / L.
[0051] Preferably, the complexing agent is one or more of ammonia water, oxalic acid and carbonate; the concentration of the complexing agent is 4-6 mol / L.
[0052] In practical applications, the concentration of the alkali solution and the concentration of the complexing agent can be adjusted according to demand. In a specific embodiment of the present invention, the concentration of the alkali solution can be 8mol / L, 9mol / L, or 10mol / L; the concentration of the complexing agent can be 4mol / L, 5mol / L, or 6mol / L.
[0053] In a second aspect, a quaternary precursor material is prepared by the above-mentioned preparation method; the chemical formula of the quaternary precursor material is Ni x Fe y Mn z Cu u (OH)2, where 0.29≤x≤0.31, 0.33≤y≤0.35, 0.31≤z≤0.33, 0.03≤u≤0.05, and x+y+z+u=1.
[0054] Preferably, the quaternary precursor material is spherical in shape and has uniform particle distribution.
[0055] In a third aspect, a method for preparing a positive electrode material is provided, which comprises mixing the above-mentioned quaternary precursor material and a sodium source, and sintering to obtain a nickel-iron-manganese-copper quaternary positive electrode material; wherein the sintering comprises three stages of sintering, and the sintering temperature of the three stages of sintering gradually increases.
[0056] The nickel-iron-manganese-copper quaternary precursor is mixed with sodium carbonate to form a hard sphere, which is then sintered in an oxygen atmosphere. Through three stages of sintering, the sintering temperature is successively increased so that the hard sphere can be heated evenly, which is beneficial to the migration of sodium ions during the working process of the positive electrode material and can improve the cycle performance and rate performance.
[0057] Preferably, the sintering temperature of the first stage sintering is 300-500° C., and the sintering time is 60-120 min.
[0058] Preferably, the sintering temperature of the second stage sintering is 550-700° C., and the sintering time is 170-230 min.
[0059] Preferably, the sintering temperature of the third stage sintering is 700-950° C., and the sintering time is 15-20 hours.
[0060] Preferably, the sodium source is one or more of sodium carbonate, sodium bicarbonate and sodium oxalate.
[0061] Preferably, the mass ratio of the quaternary precursor material to the sodium source is 1:1.02-1.04.
[0062] In order to make the technical problems to be solved, technical solutions and technical advantages of the present invention more clear, they will be described in detail below with reference to specific examples, but the protection scope of the present invention is not limited to the following specific embodiments.
[0063] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0064] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0065] Embodiment 1:
[0066] A method for preparing a quaternary precursor material comprises the following steps:
[0067] Step 1, prepare a copper ammonia solution: add 2.63 kg of copper sulfate solid into 7 mol / L ammonia water, dilute to 39.6 L to completely dissolve, and prepare a copper ammonia solution.
[0068] Prepare mixed solution A: Take 21.23 kg, 23.50 kg and 15.19 kg of nickel sulfate, ferrous sulfate and manganese sulfate respectively, add hot water to make the volume to 120 L and stir well to prepare a nickel-iron-manganese mixed solution.
[0069] Prepare the reaction kettle bottom liquid: add pure water, ammonia water and sodium hydroxide solution into the reaction kettle to prepare a reaction kettle bottom liquid with a volume of 30 L, and adjust the pH value of the reaction kettle bottom liquid to 10.7.
[0070] Step 2: Into the reactor, copper ammonia solution was introduced at 0.33 L / h, mixed solution A was introduced at 1 L / h, 5 mol / L ammonia water was introduced at 167 mL / h, and 9 mol / L sodium hydroxide solution was introduced at 400 mL / h. The pH of the reaction system was maintained at 10.7 and the temperature was maintained at 50°C. The mixture was stirred at 800 rpm for 120 h under a nitrogen atmosphere to obtain a crude precursor.
[0071] Step 3, filter the crude precursor, dry at 120°C for 36h, and obtain the quaternary precursor material Ni 0.3 Fe 0.34 Mn 0.32 Cu 0.04 (OH)2.
[0072] Comparative Example 1:
[0073] Step 1, prepare copper sulfate solution: add 2.63 kg of copper sulfate solid to 39.6 L of hot water to completely dissolve it and prepare copper sulfate solution.
[0074] Prepare mixed salt solution A: Take 21.23 kg, 23.50 kg, and 15.19 kg of nickel salt, iron salt, and manganese salt respectively, add hot water to make the volume to 120 L, stir well, and prepare mixed solution A;
[0075] Prepare the bottom liquid of the reactor: prepare the bottom liquid of the reactor by adding pure water, ammonia water and sodium hydroxide solution into the reactor to prepare a bottom liquid with a volume of 30 L, and adjust the pH value of the solution to 10.7.
[0076] Step 2: Add copper sulfate solution at 0.5 L / h, mixed solution A at 1.5 L / h, 5 mol / L ammonia water at 167 mL / h, and 9 mol / L sodium hydroxide solution at 400 mL / h into the reactor, maintain the pH of the reaction system at 10.7 and the temperature at 50°C, and stir at 800 rpm for 120 h under a nitrogen atmosphere to obtain a crude precursor.
[0077] Step 3, filter the crude precursor, dry at 120 ° C for 36 h, and obtain Ni 0.3 Fe 0.34 Mn 0.32 Cu 0.04 (OH)2 quaternary precursor material.
[0078] Figure 1 and Figure 2 The SEM images of the precursors prepared in Example 1 and Comparative Example 1 are shown in Figure 2. Figure 1 and Figure 2 It can be seen that the precursor material prepared in Example 1 of the present invention is spherical, the particle distribution is more uniform, and there is no agglomeration phenomenon.
[0079] Embodiment 2:
[0080] A method for preparing a quaternary precursor material comprises the following steps:
[0081] Step 1, prepare a copper ammonia solution: add 3.07 kg of copper sulfate solid into 7 mol / L ammonia water, dilute to 46.2 L to completely dissolve, and prepare a copper ammonia solution.
[0082] Prepare mixed solution A: Take 4.77 kg, 27.42 kg and 17.72 kg of nickel chloride, ferrous chloride and manganese chloride respectively, add hot water to make the volume to 140 L and stir well to prepare a nickel-iron-manganese mixed solution.
[0083] Prepare the bottom liquid of the reactor. Add pure water, ammonia water and sodium hydroxide solution into the reactor to prepare a bottom liquid with a volume of 30 L, and adjust the pH value of the solution to 10.2.
[0084] Step 2: Into the reactor, 0.33 L / h of copper ammonia solution, 1 L / h of mixed solution A, 222 mL / h of 4 mol / L ammonia water, and 444 mL / h of 8 mol / L sodium hydroxide solution were introduced. The pH of the reaction system was maintained at 10.7 and the temperature was maintained at 40°C. The mixture was stirred at 800 rpm for 100 h under a nitrogen atmosphere to obtain a crude precursor.
[0085] Step 3, filter the crude precursor, dry at 110°C for 48h, and obtain the quaternary precursor material Ni 0.29 Fe 0.35 Mn 0.31 Cu 0.05 (OH)2.
[0086] Embodiment 3:
[0087] A method for preparing a quaternary precursor material comprises the following steps:
[0088] Step 1, prepare a copper ammonia solution: add 2.6 kg of copper sulfate solid into 7 mol / L ammonia water, dilute to 39.6 L to completely dissolve, and prepare a copper ammonia solution.
[0089] Prepare mixed solution A: Take 23.71 kg, 15.61 kg and 19.88 kg of nickel nitrate, ferrous nitrate and manganese nitrate respectively, add hot water to make the volume to 120 L and stir well to prepare a nickel-iron-manganese mixed solution.
[0090] Prepare the bottom liquid of the reactor. Add pure water, ammonia water and sodium hydroxide solution into the reactor to prepare a bottom liquid with a volume of 30 L, and adjust the pH value of the solution to 11.1.
[0091] Step 2: Add 0.33 L / h of copper ammonia solution, 1 L / h of mixed solution A, 111 mL / h of 6 mol / L ammonia water, and 333 mL / h of 10 mol / L sodium hydroxide solution into the reactor, maintain the pH of the reaction system at 11.1, and react at 60° C. for 100 h to obtain a crude precursor.
[0092] Step 3, filter the crude precursor, dry at 130°C for 30h, and obtain the quaternary precursor material Ni 0.31 Fe 0.33 Mn0.33 Cu 0.03 (OH)2.
[0093] Embodiment 4:
[0094] A method for preparing a positive electrode material comprises the following steps:
[0095] Step 1: Take 100g of the quaternary precursor material prepared in Example 1 and 120.2g of sodium carbonate and mix them evenly. Sinter the mixed powder at 400°C for 90min, then heat it to 630°C for 200min, and then heat it to 820°C for 18h.
[0096] Step 2, cooling and grinding, Na[Ni 0.3 Fe 0.34 Mn 0.32 Cu 0.04 ]O2 positive electrode material.
[0097] Embodiment 5:
[0098] A method for preparing a positive electrode material comprises the following steps:
[0099] Step 1: Take 100 g of the quaternary precursor material Ni prepared in Example 2. 0.29 Fe 0.35 Mn 0.31 Cu 0.05 (OH)2 and 94.4g sodium bicarbonate were mixed evenly, and the mixed powder was sintered at 300℃ for 60min, then heated to 550℃ for 170min, and then heated to 700℃ for 15h.
[0100] Step 2: cooling and grinding to obtain Na[Ni 0.29 Fe 0.35 Mn 0.31 Cu 0.05 ]O2 positive electrode material.
[0101] Embodiment 6:
[0102] A method for preparing a positive electrode material comprises the following steps:
[0103] Step 1: Take 100 g of the quaternary precursor material Ni prepared in Example 2. 0.29 Fe 0.35 Mn 0.31 Cu 0.05 (OH)2 and 153.5g sodium oxalate were mixed evenly, and the mixed powder was sintered at 500℃ for 120min, then heated to 700℃ for 130min, and then heated to 950℃ for 20h.
[0104] Step 2: cooling and grinding to obtain Na[Ni0.29 Fe 0.35 Mn 0.31 Cu 0.05 ]O2 positive electrode material.
[0105] Comparative Example 2:
[0106] A method for preparing a positive electrode material comprises the following steps:
[0107] Step 1: Take 100 g of the quaternary precursor material Ni prepared in Comparative Example 1. 0.3 Fe 0.34 Mn 0.32 Cu 0.04 (OH)2 and 120.2g sodium carbonate were mixed evenly, and the mixed powder was sintered at 400℃ for 90min, then heated to 630℃ for 200min, and then heated to 820℃ for 18h.
[0108] Step 2: cooling and grinding to obtain Na[Ni 0.3 Fe 0.34 Mn 0.32 Cu 0.04 ]O2 positive electrode material.
[0109] Comparative Example 3:
[0110] A method for preparing a positive electrode material comprises the following steps:
[0111] Step 1: Take 100 g of the quaternary precursor material Ni prepared in Example 1. 0.3 Fe 0.34 Mn 0.32 Cu 0.04 (OH)2 and 120.2g sodium carbonate were mixed evenly, the mixed powder was sintered at 400℃ for 90min, then heated to 820℃ for 18h, cooled and ground to obtain Na[Ni 0.3 Fe 0.34 Mn 0.32 Cu 0.04 ]O2 positive electrode material.
[0112] Comparative Example 4:
[0113] A method for preparing a positive electrode material comprises the following steps:
[0114] Step 1: Take 100 g of the quaternary precursor material Ni prepared in Example 1. 0.3 Fe 0.34 Mn 0.32 Cu 0.04 (OH)2 and 120.2g sodium carbonate were mixed evenly, and the mixed powder was sintered at 820℃ for 18h to obtain Na[Ni 0.3 Fe0.34 Mn 0.32 Cu 0.04 ]O2 positive electrode material.
[0115] Comparative Example 5:
[0116] A method for preparing a positive electrode material comprises the following steps:
[0117] Step 1: Take 100 g of the quaternary precursor material Ni prepared in Comparative Example 1. 0.3 Fe 0.34 Mn 0.32 Cu 0.04 (OH)2 and 120.2g sodium carbonate were mixed evenly, the mixed powder was sintered at 820℃ for 18h, cooled and ground to obtain Na[Ni 0.3 Fe 0.34 Mn 0.32 Cu 0.04 ]O2 positive electrode material.
[0118] XRD (X-ray diffraction) tests were performed on the nickel-iron-manganese-copper quaternary positive electrode materials prepared in Examples 4 to 6 and Comparative Examples 2 to 5, respectively, and the values of the lattice parameters c / a of the materials were calculated. The test results are shown in Table 1 below.
[0119] Table 1 - XRD test data of nickel-iron-manganese-copper quaternary positive electrode materials prepared in Examples 4 to 6 and Comparative Examples 2 to 5
[0120]
[0121] During the charge and discharge process, the higher the c / a value, the easier it is for sodium ions to migrate. Combined with the data in Table 1, it can be seen that the c / a values of the positive electrode materials prepared in Examples 4 to 6 are higher than the c / a values of the positive electrode materials prepared in Comparative Examples 3 to 5. It can be reasonably predicted that the cycle performance and rate performance of the nickel-iron-manganese-copper quaternary positive electrode material prepared by the three-stage sintering process are more excellent. The c / a value of the positive electrode material prepared in Example 4 is greater than the c / a value of the positive electrode material prepared in Comparative Example 2, and the c / a value of the positive electrode material prepared in Comparative Example 2 is greater than the c / a value of the positive electrode material prepared in Comparative Example 5, which can explain to a certain extent that the precursor prepared by the method for preparing a precursor provided by the present invention has better performance.
[0122] The positive electrode materials prepared in Examples 4 to 6 and Comparative Examples 2 to 4 were assembled into batteries, and their material properties were tested in the following manner.
[0123] Cycle test method: The positive electrode materials prepared from the precursors prepared in Examples 4 to 6 and Comparative Examples 2 to 4 were assembled into batteries for testing using a blue electric tester. The voltage range was 2.0 to 4.3 V. The battery was activated by charging and discharging at 0.1 C for one cycle. Then, the battery was charged at a constant current and constant voltage of 0.5 C, the cut-off current was 0.05 C, and the battery was discharged at a constant current of 0.5 C for 50 cycles. The test results are shown in the figure. Figure 1 shown.
[0124] Rate test method: Use a blue electric tester to test the positive electrode materials prepared in Examples 4 to 6 and Comparative Examples 2 to 4 assembled into batteries, with a voltage range of 2.0 to 4.3V, and perform constant current and constant voltage charging at a current of 0.5C, with a charging cut-off current of 0.05C; perform constant current discharge at currents of 0.1C, 0.2C, 0.5C, 1C, 5C, 10C, and 0.1C, respectively, with a discharge cut-off voltage of 2V. The test results are as follows: Figure 2 shown.
[0125] Figure 3 It is a comparison chart of the cycle performance test results of batteries assembled with the positive electrode materials prepared in Examples 4 to 6 and Comparative Examples 2 to 4, with a current density of 0.1C. The first discharge capacity of Example 4 reaches 126 mAh / g, and after 50 cycles, it still has 125 mAh / g, with a capacity retention rate of 99%.
[0126] Figure 4 It is a comparison chart of the rate performance test results of the positive electrode materials prepared in Examples 4 to 6 and Comparative Examples 2 to 4 assembled into batteries. The current density is 0.1C, and the first discharge capacity of Example 4 reaches 122mAh / g. When the current density is increased to 10C, the capacity is still maintained at 118mAh / g. After the next cycle at 0.1C, the capacity is 124mAh / g.
[0127] Depend on Figure 3 and Figure 4 It can be seen that the first discharge capacity, cycle capacity, and capacity retention rate of the battery assembled from the positive electrode material prepared in Example 4 are all higher than those of the battery assembled from the positive electrode material prepared in Comparative Example 2, further confirming that the performance of the precursor prepared by the process for preparing the precursor provided by the present invention is superior. Comparison of the batteries assembled from the positive electrode materials prepared in Examples 4 to 6 and Comparative Examples 3 to 4 proves that the process for preparing the positive electrode material provided by the present invention can improve the cycle performance and rate performance of the positive electrode material.
[0128] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a quaternary precursor material, characterized in that: The steps include: Step 1, adding nickel salt, iron salt and manganese salt into water to obtain a mixed solution A; Step 2, introducing sodium hydroxide solution, copper ammonia solution, mixed solution A, and complexing agent into the bottom liquid of the reaction kettle, reacting for a period of time, filtering, and drying to obtain a quaternary precursor material; The temperature of the reaction system is 50~70°C, and the reaction time is 120~140h; The raw materials for preparing the copper ammonia solution include copper sulfate solution and ammonia water; The chemical formula of the prepared quaternary precursor material is Ni x Fe y Mn z Cu u (OH)2, where 0.29≤x≤0.31, 0.33≤y≤0.35, 0.31≤z≤0.33, 0.03≤u≤0.05, and x+y+z+u=1.
2. The method for preparing the quaternary precursor material according to claim 1, characterized in that: The nickel salt is one or more of nickel sulfate, nickel chloride, and nickel nitrate; the iron salt is one or more of ferrous sulfate, ferrous chloride, and ferrous nitrate; and the manganese salt is one or more of manganese sulfate, manganese chloride, and manganese nitrate.
3. The method for preparing the quaternary precursor material according to claim 1 or 2, characterized in that: The raw materials for preparing the reactor bottom liquid include sodium hydroxide solution and a complexing agent.
4. The method for preparing the quaternary precursor material according to claim 1, characterized in that: In the mixed solution A and the cuprammonia solution, the molar ratio of nickel, iron, manganese and copper is 0.29-0.31:0.33-0.35:0.31-0.33:0.03-0.05, and the sum of the molar ratios of nickel, iron, manganese and copper is 1.
5. The method for preparing the quaternary precursor material according to claim 1 or 4, characterized in that: The pH value of the reaction system is 10.2~11.
1.
6. The method for preparing a quaternary precursor material according to claim 1, characterized in that: The quaternary precursor material is spherical in shape, and the particles are evenly distributed.
7. A method for preparing a positive electrode material, characterized in that: The quaternary precursor material described in any one of claims 1 to 6 and a sodium source are mixed, and the mixture is sintered in an oxygen atmosphere to obtain a nickel-iron-manganese-copper quaternary positive electrode material; wherein the sintering includes three stages of sintering, and the sintering temperatures of the three stages of sintering gradually increase; the sintering temperature of the first stage of sintering is 300-500°C, and the sintering time is 60-120 min; the sintering temperature of the second stage of sintering is 550-700°C, and the sintering time is 170-230 min; the sintering temperature of the third stage of sintering is 700-950°C, and the sintering time is 15-20 h.
8. The method for preparing a positive electrode material according to claim 7, characterized in that: The mass ratio of the quaternary precursor material to the sodium source is 1:1.02-1.04.