A sound insulation and heat preservation fireproof board and its preparation method and application
By combining silicate cement and other materials with nanomaterial modified fillers, building panels with good sound insulation, thermal insulation and fire resistance are prepared, which solves the shortcomings of existing building materials in sound insulation, thermal insulation and fire resistance, and improves the construction Quiet and energy efficiency, and utilizes industrial waste.
Patent Information
- Application Number
- CN202410402160.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-01-19
AI Technical Summary
Existing building materials have poor effects in sound insulation, insulation and fire protection, resulting in increased noise propagation and energy consumption. It is difficult to meet sound insulation and fire protection requirements in high-rise buildings. At the same time, the insulation effect affects the stability of indoor temperature.
The sound insulation and heat-proof fire plate is prepared by reacting materials such as silicate cement, modified fillers, ceramic waste slag, fly ash, epoxy resin and curing agent. The nano-antimonium trioxide, nano-yttria, diphenyl dihydroxysilane and Modification of components such as 2-carboxyethylphenylphosphoric acid enhances component compatibility and dispersion uniformity, and forms a plate with good sound insulation, thermal insulation and fire resistance.
It realizes a board with good sound insulation, thermal insulation and fire resistance, reduces noise propagation and energy consumption, improves the quietness and safety of the building, and effectively utilizes industrial waste.
Abstract
Description
[0001] This application is a divisional application of an application with an application date of January 19, 2024, application number 202410082700.3, and invention name “A sound insulation, heat preservation and fireproof board, and its preparation method and application”. Technical Field
[0002] The invention belongs to the technical field of building materials, and in particular relates to a sound insulation, heat preservation and fireproof board and a preparation method and application thereof. Background Art
[0003] With the development of society, high-rise buildings are everywhere, resulting in the close distance between rooms. Door panels or walls with poor sound insulation make private rooms less noise-proof, affecting personal rest. At the same time, residents living on high floors find it difficult to escape in time if a fire occurs, so higher requirements are placed on the fireproof effect of door panels or walls.
[0004] In addition, in hot summer, if the door panels or walls are not well insulated, it is easy for outdoor heat to be transferred to the room through the poorly insulated walls or door panels, making the air conditioning cooling effect poor. Conversely, in winter, indoor heating heat is easily lost through poorly insulated walls or door panels, especially in high latitudes, where the outdoor temperature can reach minus 40 degrees Celsius, and indoor heating heat is easily lost, increasing energy consumption.
[0005] Therefore, it is urgent to provide a fireproof board with good sound insulation and heat preservation. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a sound insulation, heat preservation and fireproof board and a preparation method and application thereof. The sound insulation, heat preservation and fireproof board of the present invention has good sound insulation, heat preservation and fireproof effects at the same time, and is particularly suitable for buildings with low temperatures in winter and high temperatures in summer, and buildings that require good sound insulation effects. The sound insulation, heat preservation and fireproof board of the present invention is used as a door panel or a wall panel to obtain a quiet and safe indoor environment, which can provide a good living and working environment for humans.
[0007] The sound insulation and heat preservation fireproof board of the present invention is obtained by reacting a specific amount of silicate cement, modified filler, ceramic waste residue, fly ash, epoxy resin, curing agent and water. Among them, the modified filler is obtained by modifying nano antimony trioxide, nano yttrium oxide, diphenyl dihydroxy silane, 2-carboxyethyl phenyl hypophosphite and nano montmorillonite with specific organic matter (polyethylene glycol, silane coupling agent, polyacrylate) in a solvent environment of water and propylene glycol (polyethylene glycol, silane coupling agent and polyacrylate are used as modifying substances, and the silane coupling agent is hydrolyzed in a water-containing solvent, thereby playing a role in modifying organic and inorganic components, thereby enhancing the compatibility of organic and inorganic components. Polyethylene glycol and polyacrylate have a modifying effect on inorganic components, such as nano antimony trioxide and nano yttrium oxide, and improve the dispersion uniformity of nano antimony trioxide and nano yttrium oxide). The flame retardant components diphenyl dihydroxysilane and 2-carboxyethyl phenyl hypophosphorous acid are used in combination with nano antimony trioxide and nano yttrium oxide, and are modified together with polyethylene glycol, silane coupling agent and polyacrylate in the environment of water and glycerol, so that the obtained modified filler has good sound insulation, heat preservation and fire prevention effects. In particular, when the modified filler is mixed with silicate cement, ceramic waste residue, mica powder and fly ash, it is beneficial to improve the compatibility of each component, so that each component is evenly dispersed and stable, and finally the sound insulation and heat preservation fireproof board has good sound insulation, heat preservation and fire prevention effects. The sound insulation and heat preservation fireproof board of the present invention makes full use of ceramic waste residue and fly ash industrial waste to play the role of turning waste into treasure.
[0008] A first aspect of the present invention provides a sound insulation, heat preservation and fireproof board.
[0009] Specifically, a sound insulation and heat preservation fireproof board, the raw material components of which, by weight, include 100 parts of silicate cement, 3-12 parts of modified filler, 20-50 parts of ceramic waste residue, 10-15 parts of fly ash, 8-20 parts of epoxy resin, 1-5 parts of curing agent, and 30-70 parts of water;
[0010] The process of preparing the modified filler is: mixing nano antimony trioxide, nano yttrium oxide, diphenyl dihydroxy silane, 2-carboxyethyl phenyl hypophosphorous acid and nano montmorillonite, then adding polyethylene glycol, silane coupling agent, solvent and polyacrylate, mixing and dispersing, and then drying to obtain the modified filler.
[0011] Preferably, the process for preparing the modified filler is: mixing nano antimony trioxide, nano yttrium oxide, diphenyl dihydroxy silane, 2-carboxyethyl phenyl hypophosphorous acid, and nano montmorillonite in a weight ratio of 1: (0.5-3): (3-10): (2-8): (0.5-2), then adding polyethylene glycol, silane coupling agent, solvent, and polyacrylate, wherein the weight ratio of polyethylene glycol, silane coupling agent, solvent, polyacrylate to nano antimony trioxide is (4-13): (3-12): (30-50): (8-20): 1, mixing and dispersing at a speed of 2000-4000 rpm for 0.5-1.5 hours, and then vacuum drying to obtain the modified filler; the solvent includes water and glycerol.
[0012] Further preferably, the process for preparing the modified filler is: mixing nano antimony trioxide, nano yttrium oxide, diphenyl dihydroxy silane, 2-carboxyethyl phenyl hypophosphorous acid, and nano montmorillonite in a weight ratio of 1: (1.5-2.5): (4-8): (3-6): (0.5-1.5), and then adding polyethylene glycol, silane coupling agent, solvent, and polyacrylate, wherein the weight ratio of polyethylene glycol, silane coupling agent, solvent, polyacrylate to nano antimony trioxide is (5-10): (5-10): (30-40): (10-20): 1, mixing and dispersing, and then vacuum drying to obtain the modified filler; the solvent includes water and propylene glycol.
[0013] Preferably, in the solvent, the weight ratio of water to glycerol is 1:(0.8-1.5).
[0014] Preferably, the raw material components further include a water reducer, such as a polycarboxylate water reducer.
[0015] Preferably, the chemical composition of the ceramic waste includes SiC, SiO2, Al2O3, Fe2O3, TiO2, MnO2, and CaO.
[0016] Preferably, the chemical composition of the ceramic waste also includes K2O and Na2O.
[0017] Preferably, the chemical composition of the ceramic waste, by mass fraction, includes: 10-30% SiC, 25-40% SiO2, 15-22% Al2O3, 0.5-4.5% Fe2O3, 0.2-1.5% TiO2, 0.5-2.8% MnO2, 4-8% MgO, 0-1.6% CaO, 0-1.6% K2O, and 0-1.5% Na2O.
[0018] Preferably, the epoxy resin includes bisphenol A epoxy resin and bisphenol F epoxy resin.
[0019] Preferably, the curing agent is selected from at least one of ethylenediamine, diethylenetriamine, triethylenetetramine and tetraethylenepentamine.
[0020] Preferably, the raw material components further include hydroxy polydimethylsiloxane and mica powder modified by a silane coupling agent.
[0021] Preferably, the preparation process of the mica powder modified by hydroxy polydimethylsiloxane and silane coupling agent is as follows: hydroxy polydimethylsiloxane, silane coupling agent, mica powder, water and glycerol are mixed and dispersed at a speed of 1000-3000 rpm and 40-55° C. for 1-3 hours, and then dried to obtain the mica powder modified by hydroxy polydimethylsiloxane and silane coupling agent. After modification, the mica powder can improve the compatibility with other components and help improve the sound insulation and heat insulation effects of sound insulation and fireproof boards.
[0022] Preferably, the preparation process of the mica powder modified by hydroxy polydimethylsiloxane and silane coupling agent is as follows: hydroxy polydimethylsiloxane, silane coupling agent, mica powder, water and glycerol are mixed and dispersed in a weight ratio of 5: (5-15): (3-8): (10-25): (8-15), and the mixing and dispersion is carried out at a speed of 1000-3000 rpm and 40-55° C. for 1-3 hours, and then dried to obtain the mica powder modified by hydroxy polydimethylsiloxane and silane coupling agent.
[0023] Preferably, the silane coupling agent is selected from KH560 and / or KH570.
[0024] Preferably, the thickness of the sound insulation, heat preservation and fireproof board is 30-90 mm, for example, 30 mm, 40 mm, 50 mm, 60 mm, 70 mm, 80 mm, 90 mm.
[0025] Preferably, a sound insulation, heat preservation and fireproof board, the raw material components of which, by weight, include 100 parts of silicate cement, 3-12 parts of modified filler, 20-50 parts of ceramic waste slag, 10-15 parts of fly ash, 8-20 parts of epoxy resin, 1-5 parts of curing agent, 30-70 parts of water, and 5-10 parts of mica powder modified by hydroxy polydimethylsiloxane and silane coupling agent.
[0026] More preferably, a sound insulation, heat preservation and fireproof board, whose raw material components, by weight, include 100 parts of silicate cement, 5-12 parts of modified filler, 20-40 parts of ceramic waste slag, 10-12 parts of fly ash, 8-15 parts of epoxy resin, 1-5 parts of curing agent, 30-60 parts of water, 5-10 parts of mica powder modified by hydroxy polydimethylsiloxane and silane coupling agent, and 5-10 parts of water reducer.
[0027] A second aspect of the present invention provides a method for preparing a sound insulation, heat preservation and fireproof board.
[0028] Specifically, a method for preparing a sound insulation and heat preservation fireproof board comprises the following steps:
[0029] Weigh each raw material component, then stir and mix silicate cement, modified filler, ceramic waste slag, fly ash, epoxy resin, then add curing agent and water, continue to stir and mix to obtain a mixture, add the mixture into a mold, then solidify and shape, demould, and maintain to obtain the sound insulation and heat preservation fireproof board.
[0030] Preferably, the hydroxy polydimethylsiloxane and the mica powder modified by the silane coupling agent are added simultaneously when the fly ash is added.
[0031] Preferably, the mesh size of the ceramic waste slag and fly ash is 100-300 mesh, for example, 100 mesh, 200 mesh, or 300 mesh.
[0032] Preferably, the curing conditions are: temperature of 20-40° C., relative humidity of 65-85%, and curing time of 24-48 hours.
[0033] Preferably, the curing conditions are: temperature of 20-40° C., relative humidity of 65-85%, and curing time of 24-48 hours.
[0034] A third aspect of the present invention provides an application of a sound insulation, heat preservation and fireproof board.
[0035] Application of the above-mentioned sound insulation, heat preservation and fireproof board in the field of construction.
[0036] A door panel comprises the above-mentioned sound insulation, heat preservation and fireproof panel.
[0037] A wall panel comprises the above-mentioned sound insulation, heat preservation and fireproof panel.
[0038] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0039] (1) The sound insulation and heat preservation fireproof board of the present invention is obtained by reacting specific amounts of silicate cement, modified filler, ceramic waste residue, fly ash, epoxy resin, curing agent and water. Among them, the modified filler is obtained by modifying nano antimony trioxide, nano yttrium oxide, diphenyl dihydroxy silane, 2-carboxyethyl phenyl hypophosphite and nano montmorillonite with specific organic matter (polyethylene glycol, silane coupling agent, polyacrylate) in a solvent environment of water and glycerol. The flame retardant components diphenyl dihydroxysilane and 2-carboxyethyl phenyl hypophosphorous acid are used in combination with nano antimony trioxide and nano yttrium oxide, and are modified together with polyethylene glycol, silane coupling agent and polyacrylate in the environment of water and glycerol, so that the obtained filler has good sound insulation, heat preservation and fire prevention effects. In particular, when the modified filler is mixed with silicate cement, ceramic waste residue, mica powder and fly ash, it is beneficial to improve the compatibility of each component, so that each component is evenly dispersed and stable, and finally the sound insulation and heat preservation fireproof board has good sound insulation, heat preservation and fire prevention effects. The sound insulation and heat preservation fireproof board of the present invention makes full use of ceramic waste residue and fly ash industrial waste to play the role of turning waste into treasure.
[0040] (2) The raw material components of the sound insulation, heat preservation and fireproof board of the present invention also include hydroxy polydimethylsiloxane and mica powder modified by silane coupling agent. After the mica powder is modified, its compatibility with other components can be improved, and it is helpful to improve the sound insulation and heat preservation effect of the sound insulation, heat preservation and fireproof board. DETAILED DESCRIPTION
[0041] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0042] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0043] The silicate cement used in the following examples and comparative examples is commercially available ordinary silicate cement PO32.5.
[0044] Example 1: Preparation of sound insulation and fireproof board
[0045] A sound insulation and heat preservation fireproof board, the raw material components of which, by weight, are 100 parts of silicate cement, 10 parts of modified filler, 25 parts of ceramic waste slag, 15 parts of fly ash, 10 parts of epoxy resin (5 parts of bisphenol A epoxy resin, 5 parts of bisphenol F epoxy resin), 4 parts of curing agent (2 parts of diethylenetriamine, 2 parts of triethylenetetramine), 1 part of polycarboxylic acid water reducer, and 60 parts of water;
[0046] The chemical composition of ceramic waste slag is: 30% SiC, 37.5% SiO2, 20% Al2O3, 3.5% Fe2O3, 1% TiO2, 2.0% MnO2, 5% MgO, 0.5% CaO, 0.3% K2O, 0.2% Na2O;
[0047] The process for preparing the modified filler is as follows: nano antimony trioxide, nano yttrium oxide, diphenyl dihydroxy silane, 2-carboxyethyl phenyl hypophosphorous acid and nano montmorillonite are mixed in a weight ratio of 1:1:4:3:1, and then polyethylene glycol 4000, silane coupling agent KH560, solvent and polyacrylate are added, wherein the weight ratio of polyethylene glycol 4000, silane coupling agent KH560, solvent (the solvent is composed of water and propylene glycol in a weight ratio of 1:1), polyacrylate and nano antimony trioxide is 5:5:40:10:1, and the mixture is mixed and dispersed at a speed of 3000 rpm for 1 hour, and then vacuum dried to obtain the modified filler.
[0048] The thickness of the sound insulation and heat preservation fireproof board is 80mm.
[0049] A method for preparing a sound insulation and heat preservation fireproof board comprises the following steps:
[0050] Weigh each raw material component, then stir and mix silicate cement, modified filler, ceramic waste, fly ash, epoxy resin, at a stirring speed of 800 rpm, for 1 hour, then add curing agent and water, continue to stir and mix, at a stirring speed of 800 rpm, for 10 minutes, to obtain a mixture, add the mixture into a mold, and then cure and shape it (temperature is 30°C, relative humidity is 85%, and curing time is 36 hours), demold, and cure (temperature is 25°C, relative humidity is 80%, and curing time is 48 hours) to obtain a sound insulation and heat preservation fireproof board.
[0051] Example 2: Preparation of sound insulation and fireproof board
[0052] A sound insulation and heat preservation fireproof board, the raw material components of which, by weight, are 100 parts of silicate cement, 5 parts of modified filler, 20 parts of ceramic waste residue, 10 parts of fly ash, 12 parts of epoxy resin (6 parts of bisphenol A epoxy resin, 6 parts of bisphenol F epoxy resin), 5 parts of curing agent (2 parts of diethylenetriamine, 3 parts of triethylenetetramine), and 70 parts of water;
[0053] The chemical composition of the ceramic waste residue, by mass fraction, is: 30% SiC, 35.5% SiO2, 20% Al2O3, 3.5% Fe2O3, 1% TiO2, 2.0% MnO2, 7% MgO, 0.5% CaO, 0.3% K2O, 0.2% Na2O;
[0054] The process for preparing the modified filler is as follows: nano antimony trioxide, nano yttrium oxide, diphenyl dihydroxy silane, 2-carboxyethyl phenyl hypophosphorous acid and nano montmorillonite are mixed in a weight ratio of 1:2:8:3:1.2, and then polyethylene glycol 6000, silane coupling agent KH570, solvent and polyacrylate are added, wherein the weight ratio of polyethylene glycol 6000, silane coupling agent KH570, solvent (the solvent is water and propylene glycol in a weight ratio of 1:1.1), polyacrylate and nano antimony trioxide is 5:8:35:12:1, the mixture is mixed and dispersed at a speed of 4000 rpm for 1 hour, and then vacuum dried to obtain the modified filler.
[0055] The thickness of the sound insulation and heat preservation fireproof board is 80mm.
[0056] A method for preparing a sound insulation and heat preservation fireproof board comprises the following steps:
[0057] Weigh each raw material component, then stir and mix silicate cement, modified filler, ceramic waste, fly ash, epoxy resin, at a stirring speed of 1000 rpm, for 1 hour, then add curing agent and water, continue to stir and mix, at a stirring speed of 1000 rpm, for 15 minutes, to obtain a mixture, add the mixture into a mold, then cure and shape (temperature is 25°C, relative humidity is 80%, and curing time is 48 hours), demold, and cure (temperature is 30°C, relative humidity is 80%, and curing time is 48 hours) to obtain a sound insulation and heat preservation fireproof board.
[0058] Example 3: Preparation of sound insulation and fireproof board
[0059] A sound insulation and heat preservation fireproof board, the raw material components of which, by weight, are 100 parts of silicate cement, 10 parts of modified filler, 25 parts of ceramic waste slag, 15 parts of fly ash, 10 parts of epoxy resin (5 parts of bisphenol A epoxy resin, 5 parts of bisphenol F epoxy resin), 4 parts of curing agent (2 parts of diethylenetriamine, 2 parts of triethylenetetramine), 1 part of polycarboxylic acid water reducer, 60 parts of water, and 6 parts of mica powder modified by hydroxy polydimethylsiloxane and silane coupling agent;
[0060] The chemical composition of ceramic waste slag is: 30% SiC, 37.5% SiO2, 20% Al2O3, 3.5% Fe2O3, 1% TiO2, 2.0% MnO2, 5% MgO, 0.5% CaO, 0.3% K2O, 0.2% Na2O;
[0061] The process of preparing the modified filler is as follows: nano antimony trioxide, nano yttrium oxide, diphenyl dihydroxy silane, 2-carboxyethyl phenyl hypophosphorous acid, and nano montmorillonite are mixed in a weight ratio of 1:1:4:3:1, and then polyethylene glycol 4000, silane coupling agent KH560, solvent, and polyacrylate are added, wherein the weight ratio of polyethylene glycol 4000, silane coupling agent KH560, solvent (the solvent is composed of water and glycerol in a weight ratio of 1:1), polyacrylate, and nano antimony trioxide is 5:5:40:10:1, and the mixture is mixed and dispersed at a speed of 3000 rpm for 1 hour, and then vacuum dried to obtain the modified filler;
[0062] The preparation process of mica powder modified by hydroxy polydimethylsiloxane and silane coupling agent is as follows: hydroxy polydimethylsiloxane, silane coupling agent KH560, mica powder, water and propylene glycol are mixed and dispersed in a weight ratio of 5:10:5:15:10, and the mixing and dispersion is carried out at a speed of 2000 rpm and 45°C for 1.5 hours, and then vacuum dried to obtain mica powder modified by hydroxy polydimethylsiloxane and silane coupling agent.
[0063] The thickness of the sound insulation and heat preservation fireproof board is 80mm.
[0064] A method for preparing a sound insulation and heat preservation fireproof board comprises the following steps:
[0065] Weigh each raw material component, then stir and mix silicate cement, modified filler, ceramic waste, fly ash, hydroxy polydimethylsiloxane and mica powder modified by silane coupling agent, epoxy resin, at a stirring speed of 800 rpm for 1 hour, then add curing agent and water, continue to stir and mix, at a stirring speed of 800 rpm for 10 minutes, to obtain a mixture, add the mixture into a mold, then cure and shape (temperature is 30°C, relative humidity is 85%, and curing time is 36 hours), demould, and cure (temperature is 25°C, relative humidity is 80%, and curing time is 48 hours) to obtain a sound insulation and heat preservation fireproof board.
[0066] Comparative Example 1
[0067] Compared with Example 1, an equal amount of nano antimony trioxide was used to replace nano yttrium oxide in Comparative Example 1, and the rest of the process was the same as that of Example 1. That is, in the preparation process of the modified filler in Comparative Example 1, nano yttrium oxide was not used.
[0068] Comparative Example 2
[0069] Compared with Example 1, an equal amount of 2-carboxyethylphenylphosphinate was used to replace diphenyldihydroxysilane in Comparative Example 2, and the rest of the process was the same as that of Example 1. That is, in the preparation process of the modified filler in Comparative Example 2, diphenyldihydroxysilane was not used.
[0070] Comparative Example 3
[0071] Compared with Example 1, the amount of ceramic waste slag used in Comparative Example 3 is 55 parts and fly ash is 5 parts, and the other components and processes are the same as those in Example 1.
[0072] Product effect testing
[0073] The sound insulation, heat preservation and fireproof boards prepared in Example 1, Example 3 and Comparative Examples 1-3 were cured for 14 days at a temperature of 30° C. and a relative humidity of 80%. The sound absorption coefficient was tested according to the standing wave tube method, the thermal conductivity was tested according to the standard JC275-1996, and the flame retardancy was tested according to the standard GB 8624-2012. The results are shown in Table 1.
[0074] Table 1
[0075] Sound absorption coefficient (%) Thermal conductivity (W / (m·k)) Flame retardant Example 1 33 0.102 A1 Example 3 36 0.081 A1 Comparative Example 1 28 0.126 A1 Comparative Example 2 32 0.113 A2 Comparative Example 3 26 0.154 A2
[0076] It can be seen from Table 1 that the sound insulation, heat preservation and fireproof performance of the sound insulation, heat preservation and fireproof board prepared in Example 1 is significantly better than that of Comparative Examples 1-3.
[0077] It can be seen from the effect data of Comparative Example 1 that when nano antimony trioxide is used instead of nano yttrium oxide, the sound insulation and thermal insulation effects of the board are significantly reduced. The main reason is that when nano yttrium oxide is missing, the mutual coordination between nano yttrium oxide and nano antimony trioxide is missing, which affects the conduction of electrons and the dispersion of nano antimony trioxide, thereby reducing the sound insulation and thermal insulation effects of the board. Sound insulation and thermal insulation performance are closely related to the electron gain and loss or conduction function of sound insulation and thermal insulation performance. The present invention makes full use of the electron gain and loss performance of nano yttrium oxide, and cooperates with nano antimony trioxide to improve the sound insulation and thermal insulation performance of the sound insulation and thermal insulation fireproof board.
[0078] It can be seen from the effect data of Comparative Example 2 that after changing the flame retardant component, the sound insulation and heat preservation effects of the board are not greatly affected, but the flame retardant effect of the board is significantly affected. It can be seen that the present invention needs to use two specific flame retardant components at the same time to prepare the modified filler. The present invention mainly uses 2-carboxyethylphenyl hypophosphite and diphenyldihydroxysilane as flame retardant components to improve the flame retardant properties of the board. Although nano antimony trioxide also has certain flame retardancy, the main function of nano antimony trioxide in the present invention is to cooperate with the above-mentioned other components to modify so that the sound insulation and heat preservation fireproof board obtains better sound insulation and heat preservation.
[0079] It can be seen from the effect data of Comparative Example 3 that after changing the amount of ceramic waste slag and fly ash, the compatibility or dispersion uniformity of each component has a significant adverse effect, so that the sound insulation, heat preservation and fire prevention effects of the prepared board are significantly reduced. Ceramic waste slag is an industrial waste slag, which cannot be added infinitely during the utilization process. The present invention uses modified fillers and other components to increase the amount of ceramic waste slag to 50 parts, but if ceramic waste slag is continued to be added, even with the modified fillers used in the amount of Comparative Example 3 and other components in Comparative Example 3, the dispersion uniformity of each component will be significantly deteriorated, thereby significantly reducing the sound insulation, heat preservation and fire prevention effects of the sound insulation and heat preservation fireproof board.
[0080] It can be seen from the effect data of Example 1 and Example 3 that the sound insulation and heat preservation effects of the board can be significantly improved after adding hydroxy polydimethylsiloxane and mica powder modified by silane coupling agent.
[0081] In addition, the 28-day compressive strength of the sound insulation and heat preservation fireproof board prepared in Example 1 was tested according to the standard GB / T50081-2002, and the result was 25.1 MPa, which has good mechanical properties.
[0082] Application Examples
[0083] A door panel comprises the sound insulation, heat preservation and fireproof panel prepared in Example 1.
[0084] A wall panel comprises the sound insulation, heat preservation and fireproof panel prepared in Example 3.
Claims
1. A sound insulation and heat preservation fireproof board, characterized in that: The raw material components are composed of the following components by weight: 100 parts of silicate cement, 3-12 parts of modified filler, 20-50 parts of ceramic waste residue, 10-15 parts of fly ash, 8-20 parts of epoxy resin, 1-5 parts of curing agent, 30-70 parts of water, and water reducing agent; The process for preparing the modified filler is as follows: nano antimony trioxide, nano yttrium oxide, diphenyl dihydroxy silane, 2-carboxyethyl phenyl hypophosphorous acid and nano montmorillonite are mixed in a weight ratio of 1: (0.5-3): (3-10): (2-8): (0.5-2), and then polyethylene glycol, silane coupling agent, solvent and polyacrylate are added, wherein the weight ratio of polyethylene glycol, silane coupling agent, solvent, polyacrylate and nano antimony trioxide is (4-13): (3-12): (30-50): (8-20): 1, and the mixture is mixed and dispersed at a speed of 2000-4000 rpm for 0.5-1.5 hours, and then vacuum dried to obtain the modified filler; the solvent comprises water and propylene glycol.
2. The sound insulation and heat preservation fireproof board according to claim 1, characterized in that: The chemical components of the ceramic waste slag include SiC, SiO2, Al2O3, Fe2O3, TiO2, MnO2 and CaO.
3. The sound insulation and heat preservation fireproof board according to claim 1, characterized in that: The water reducer is a polycarboxylate water reducer.
4. The sound insulation and heat preservation fireproof board according to claim 1, characterized in that: The epoxy resin includes bisphenol A epoxy resin and bisphenol F epoxy resin.
5. The sound insulation and heat preservation fireproof board according to any one of claims 1 to 4, characterized in that: The thickness of the sound insulation, heat preservation and fireproof board is 30-90 mm.
6. Application of the sound insulation, heat preservation and fireproof board according to any one of claims 1 to 5 in the field of construction.
7. A door panel, characterized in that: The invention comprises the sound insulation, heat preservation and fireproof board as described in any one of claims 1 to 5.
8. A wall panel, characterized in that: The invention comprises the sound insulation, heat preservation and fireproof board as described in any one of claims 1 to 5.
Citation Information
Patent Citations
Building fireproof heat preservation plate and preparation method thereof
CN105503224A
Thermal insulation building material and preparation method thereof
CN108706926A
Sound-insulation heat-preservation fireproof plate as well as preparation method and application thereof
CN117602908A