A method for controlling axle steel calcium treatment process

By adjusting the calcium treatment amount and refining slag composition according to the Als loss during the RH process in the axle steel smelting process, combined with vacuum refining and protective casting technology, the problem of unstable calcium treatment effects is solved and the effective removal of inclusions in axle steel is achieved. Improved control and castability meet inclusion requirements for high-speed axles and increase production efficiency and cost-effectiveness.

CN118480643BActive Publication Date: 2024-10-01MAANSHAN MAGANG JINXI RAIL TRANSPORT EQUIP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410938819.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The calcium treatment effect in the existing axle steel smelting process is unstable and it is difficult to effectively control Ds inclusions, resulting in poor pourability of molten steel. Moreover, the existing method has a long smelting cycle, high cost, or is difficult to control accurately.

Method used

A calcium treatment process related to Als loss in the RH process is designed. By feeding the amount of calcium silicon wire or pure calcium wire, the amount is adjusted according to the Als loss during the RH vacuum treatment process. The calcium treatment process is controlled by combining vacuum refining and protective casting technology. processing capacity and refining slag composition to achieve effective denaturation and stable control of inclusions.

Benefits of technology

Stable control of inclusions in axle steel has been achieved. The pourability of molten steel is good, and the inclusion inspection pass rate reaches 100%. Among them, Class A, Class B, and Class D inclusions are all at or below level 1.0, and Class Ds inclusions are ≤1.0. grade, meeting the inclusion requirements of high-speed axles, and the process is suitable for efficient and economical production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118480643B_ABST
    Figure CN118480643B_ABST
Patent Text Reader

Abstract

The present invention provides a method for controlling axle steel calcium treatment process. Compared with the prior art, the present invention is conducive to controlling the refined slag system of axle steel inclusions; a calcium treatment process related to Als loss in the RH process is designed, and the feeding amount L of the silicon calcium wire is fed Si‑Ca线 =([20+1250×Δ[Als] RH ])×W s / 100±5m, feeding amount of pure calcium wire L Ca线 =([10+1875×Δ[Als] RH ])×W s / 100±5 m; Δ[Als] RH =[Als 样① ‑Als 样② ]×RH 真空 / (RH 真空 ‑3). Effective modification of inclusions is achieved, the castability of molten steel is good, and inclusions are stably and effectively controlled, meeting the control requirements of steel grades for inclusions. The first-time pass rate of inclusion inspection is 100%, among which Class B inclusions are all ≤1.0, Class D inclusions are all ≤1.5, and Class Ds inclusions are ≤1.0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of iron and steel metallurgy, and in particular relates to a method for controlling axle steel calcium treatment process. Background Art

[0002] Axles have high requirements for fatigue performance, and the types and levels of inclusions in axle steel must be strictly controlled, especially for brittle inclusions and point-shaped non-deformed inclusions in steel that can easily lead to fatigue failure of axles. At present, the axle steel smelting production process mainly adopts high-alkalinity + calcium treatment continuous casting production process. The high-alkalinity process can effectively promote the denaturation of brittle inclusions of type B in steel, and the calcium treatment process can effectively improve the castability of molten steel. The timing and effect of calcium treatment have a great influence on the control of inclusions. If the amount of calcium treatment is insufficient, the denaturation effect of inclusions is poor and the castability of molten steel is poor. Excessive calcium treatment will result in a high content of dissolved Ca in the steel, which can easily lead to excessive Ds inclusions.

[0003] A domestic steel plant adopts high basicity + RH calcium treatment continuous casting process for axle steel smelting and production. The calcium wire feeding time is to feed a fixed amount of calcium wire after RH breaks the air. Although the castability of molten steel is good after wire feeding, the calcium treatment effect is unstable, and Ds inclusions often reach above level 2.0, which is difficult to meet the requirements of high-speed axles for inclusions. The results are mainly composite inclusions mainly composed of calcium aluminates, which are endogenous inclusions in molten steel. Therefore, it is necessary to optimize the calcium treatment process to meet the control requirements of steel grades.

[0004] The patent "A smelting method for controlling silicate inclusions in axle steel" with publication number CN 115287401 A published on November 4, 2022 discloses that stable control of brittle silicate inclusions is achieved by adopting a high alkalinity + RH calcium treatment process. However, this method has a high alkalinity (R≥8) and a large amount of calcium wire feeding, which is not conducive to the control of Ds-type inclusions in steel. The patent with publication number CN 114086062 A published on February 25, 2022 discloses "A steel for high-speed railway axles and its production method", which provides a slag pouring operation before VD vacuum treatment (30~40% of refined slag is poured out), and 30~80m silicon-calcium wire is fed for calcium treatment after vacuum treatment, the inclusions are denatured, and soft blowing is strengthened (soft blowing time is 30~40min), so that the Ds-type inclusions of the axle are stably controlled below level 0.5. This method requires slag pouring. On the one hand, the smelting cycle is long, and on the other hand, the process temperature drop is large. In addition, the soft blowing time after wire feeding is long, which is not conducive to efficient and economical production. The patent with the publication number CN 106119461 A published on November 16, 2016 discloses "A method for calcium treatment of molten steel". It discloses that calcium treatment can meet the effective calcium content requirements in molten steel by adding calcium-containing alloys during the LF refining process. The operation is simple and the cost is low. However, this method is not suitable for steel types treated in vacuum. Adding under vacuum conditions is prone to splashing and cold steel in the vacuum chamber, which is not conducive to the cleanliness of molten steel. The patent with the publication number CN 105506221 A published on April 20, 2016 discloses "A method for calcium treatment of pipeline steel". This method achieves effective denaturation of inclusions by accurately controlling the composition of refined slag and determining the feeding amount by the total oxygen content and sulfur content in molten steel, reducing and inhibiting the generation of large inclusions in molten steel. However, this method has high requirements for refined slag control on the one hand, and on the other hand, the oxygen content and sulfur content in molten steel need to be accurately quantified before feeding. In particular, the quantification time of total oxygen content is long and the accuracy is poor. In the actual production and smelting process, the control window is too narrow and it is difficult to control stably and accurately. Summary of the invention

[0005] The purpose of the present invention is to provide a method for controlling the calcium treatment process of axle steel, provide a refined slag system that is beneficial to controlling the inclusions in axle steel, design a calcium treatment process related to Als loss in the RH process, achieve effective modification of inclusions, good castability of molten steel and stable and effective control of inclusions, and meet the control requirements of steel grades for inclusions.

[0006] The specific technical solutions of the present invention are as follows:

[0007] A method for controlling axle steel calcium treatment process comprises the following steps:

[0008] (1) For smelting, the molten iron entering the furnace must have a P content of ≤0.15% and a S content of ≤0.040%;

[0009] (2) Deoxidation and alloying during the steel tapping process;

[0010] (3) LF refining to adjust the composition of the refined slag;

[0011] (4) Vacuum refining, after breaking the vacuum, feed silicon calcium wire or pure calcium wire for calcium treatment;

[0012] (5) After the molten steel is put on the stage, it is left to stand for 15 to 30 minutes before pouring. Protected casting is used during the casting process;

[0013] In step (1), a converter or an electric furnace is used for smelting;

[0014] In step (1), the iron-steel ratio is controlled at 10-70%, the scrap steel is low-sulfur scrap steel, and the S content in the scrap steel is ≤0.015%;

[0015] In step (1), the endpoint control of the converter or electric furnace requires that the C content be between 0.08% and 0.25%, the P content be ≤0.013%, and the [O] content be ≤300 ppm; the endpoint temperature be between 1600 and 1680°C, the slag blocking during steel tapping be strengthened, and the slag amount be controlled to be less than 4 kg / ton of steel;

[0016] In step (2), the deoxidation alloying process uses an aluminum deoxidizer to deoxidize the molten steel and slag, and the aluminum deoxidizer is aluminum iron or aluminum particles;

[0017] In step (2), when 1 / 3 of the steel is tapped, aluminum deoxidizer, slag material and alloy are added in sequence;

[0018] In step (2), the slag-making material includes lime and pre-melted refined slag, wherein the amount of lime added is 2.5-4.5 kg / ton of steel, the amount of pre-melted refined slag added is 1.8-3.0 kg / ton of steel, and the target amount of alloy added is controlled according to the lower limit of the internal control of the steel grade; the pre-melted refined slag mainly has a CaO content of 45-55%, an Al2O3 content of 35-45%, a SiO2 content of ≤9%, a Mg content of ≤10%, and a particle size of 5-40 mm;

[0019] In step (2), the ladle is strongly stirred during the steel-discharging process, and the bottom blowing argon gas flow rate is controlled at 300-600 NL / min;

[0020] In step (3), lime, pre-melted refined slag, aluminum particles, silicon carbide, etc. are used to make refined slag. The refining process is required to make slag quickly. The refined slag composition control requirements are CaO content 40-60%, SiO2 content 8-18%, Al2O3 content 22-35%, (FeO+MnO) ≤ 1.0%, binary basicity (CaO / SiO2) is controlled at 2.5-5.0, CaO / Al2O3 ratio is controlled at 1.0-2.0, the amount of refined slag is controlled at 12-20 kg / ton steel, the refining time after slag formation is ≥ 15 min, and the LF refining cycle is controlled within 120 min;

[0021] In step (4), the vacuum refining controls the vacuum degree to ≤100Pa, the vacuum treatment cycle is more than 15min, the hydrogen content before breaking the vacuum is ≤1.0ppm, and after breaking the vacuum, a wire feeder is used to feed silicon calcium wire or pure calcium wire for calcium treatment;

[0022] In step (4), the amount of silicon calcium wire or pure calcium wire fed is based on the aluminum loss Δ[Als] during the RH vacuum treatment process. RH Determine; feed amount L of calcium silicon wire Si-Ca线 =(20+1250×Δ[Als] RH )×W s / 100±5m, feeding amount of pure calcium wire L Ca线 =(10+1875×Δ[Als] RH )×W s / 100±5 m;

[0023] Δ[Als] RH =[Als 样① -Als 样② ]×RH 真空 / (RH 真空 -3);

[0024] Where Als 样① ①Als value of the sample before RH vacuum treatment, unit: %; Als 样② It is the Als value of the sample 3 minutes before RH breaks through the air, the unit is %; RH 真空 is the RH vacuum treatment time, in min; Ws is the weight of molten steel, in t; L Si-Ca线 is the amount of calcium silicon wire fed, unit: m; L Ca线 It is the feeding amount of pure calcium wire, unit is m; when calculating with the above formula, directly bring the value before the unit into the formula calculation interface.

[0025] The present invention is based on the fact that the wire feeding amount mainly depends on the number of inclusions in the molten steel, the number of inclusions generated in the vacuum process corresponds to the Als loss in the RH vacuum process, the greater the Als loss, the greater the number of inclusions generated, and the corresponding wire feeding amount will increase, and the wire feeding amount calculation formula is obtained by fitting. In the formula, the preceding 20 and 10 are basic values, which are used for basic modification, mainly including the deoxidation products that are not removed by floating and the secondary oxidation products generated in the air-breaking process; 1250 and 1875 are values ​​calculated by fitting based on the actual wire feeding amount. ±5m is the deviation control range of the wire feeding amount.

[0026] In step (4), after calcium treatment, 150-350 kg of heat preservation agent is evenly added to the slag surface to keep it warm and inhibit secondary oxidation. After the heat preservation agent is added, the molten steel is soft-blown, and the bottom blowing flow rate is 10-50 NL / min. The top slag is kept without bright surface or slightly bright surface and slightly floating. The soft blowing time is 15-25 minutes.

[0027] In step (4), the heat preservation agent is carbonized rice husk, and the slag surface is required to be fully covered;

[0028] In step (5), the molten steel is allowed to stand for 15 to 30 minutes before pouring to promote the removal of inclusions. During the casting process, the "large ladle long shroud + medium ladle + submerged shroud" protection casting should be well done, and the Als loss should be controlled within 50ppm from the RH exit to the medium ladle sampling (when the large ladle is cast 1 / 2).

[0029] By adopting the axle steel calcium treatment process control method of the present invention, the inclusion inspection pass rate of the rolled axle steel billet reaches 100%, wherein the A-type coarse inclusions are all ≤1.0 level, the B-type coarse inclusions are all ≤1.0 level, the D-type coarse inclusions are all ≤1.5 level, and the Ds-type inclusions are ≤1.0 level.

[0030] In the present invention, the P and S of the molten iron entering the furnace are limited in order to reduce the burden of LF refining and avoid secondary oxidation caused by too long refining time; the tapping conditions are limited on the one hand to reduce the oxygen content after the primary refining furnace and reduce the generation of deoxidation products, and on the other hand to create conditions for refining; the slag making process is more conducive to the formation of refining slag with appropriate basicity and good fluidity, which is conducive to the floating removal of inclusions; the vacuum process will cause secondary oxidation of the molten steel due to secondary oxidation and the shedding of residual steel, etc., and produce inclusions, which is mainly reflected in the attenuation of Als. The greater the attenuation, the more inclusions are generated, and the more calcium wire needs to be fed for inclusion denaturation. The addition of heat preservation agent is to prevent the refining slag from crusting. Combined with the above-mentioned refining slag control and soft blowing control, the adsorption and removal of secondary oxidation products and denatured products in the air-breaking process and wire feeding process are realized. Standing during the casting process is conducive to the removal of tiny inclusions, and protecting the casting and controlling Als is mainly to prevent secondary oxidation during the casting process.

[0031] Compared with the prior art, the present invention is conducive to controlling the refined slag system of axle steel inclusions; a calcium treatment process related to Als loss in the RH process is designed to achieve effective modification of inclusions, good castability of molten steel and stable and effective control of inclusions, meeting the control requirements of steel grades for inclusions. The first-time qualified rate of inclusion inspection of rolled axle steel billets reaches 100%, among which Class B inclusions are all ≤1.0, Class D inclusions are all ≤1.5, and Class Ds inclusions are ≤1.0. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the random field inclusion morphology of the ingot of Comparative Example 2 sample 1 before process optimization;

[0033] Figure 2 This is the random field inclusion morphology of the second ingot of the sample of Example 1 after process optimization;

[0034] Figure 3 This is the random field of inclusion morphology of the three-axle sample of Comparative Example 2 before process optimization;

[0035] Figure 4 This is the random field of view inclusion morphology of the four-axle sample of Example 1 after process optimization. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Practical application case 1:

[0038] Taking the production of 110t steel by electric furnace smelting as an example, the specific production methods of each embodiment and comparative example are as follows:

[0039] (1) The steel produced in each embodiment and comparative example is axle steel IDC35e. The main components of molten steel in each heat are shown in Table 1. The remainder not shown in Table 1 is Fe and unavoidable impurities.

[0040] Table 1 Molten steel composition (intermediate composition) of each heat / %

[0041]

[0042] (2) The P content of the hot metal entering the furnace is controlled at 0.10%~0.14%, the S content is controlled at 0.021%~0.038%, and the iron-steel ratio is 35%~65%; the scrap steel is low-sulfur scrap steel, and the S content in the scrap steel is ≤0.015%;

[0043] (3) The final C content of the electric furnace is 0.12%~0.24%, the P content is 0.008%~0.012%, the final [O] content is 135~278ppm, the final temperature is 1612~1657℃, and the slag amount is about 2.0~2.9kg / ton steel;

[0044] (4) When 1 / 3 of the steel is tapped, 3.5-4.5 kg / ton of aluminum iron, 3.0-4.5 kg / ton of lime, and 1.8-2.8 kg / ton of pre-melted refined slag are added in sequence; the composition of the molten refined slag is mainly CaO content 45-55%, Al2O3 content 35-45%, SiO2 content ≤9%, Mg content ≤10%, and particle size 5-40 mm; during the tapping process, the ladle is strongly stirred (the bottom blowing argon gas flow rate is controlled at 500 NL / min);

[0045] (5) The composition of LF refining slag is CaO content 42~55%, SiO2 content 9~16%, Al2O3 content 22~35%, (FeO+MnO) is controlled at 0.3%~0.9%, binary basicity (CaO / SiO2) is controlled at 2.6~4.9, CaO / Al2O3 ratio is controlled at 1.1~1.9, the amount of refining slag is controlled at 12~19kg / ton steel, the refining time after slag formation is 16~25min, and the LF refining cycle is controlled at 58~112min;

[0046] (6) Vacuum refining vacuum degree 54~95Pa, vacuum treatment cycle 15~20min, hydrogen [H] content 0.5~0.8ppm before breaking the air, Als and feeding amount of vacuum process are shown in Table 1 below, 150~292kg of carbonized rice husks as heat preservation agent are added during breaking the air, and soft blowing time is 15~25min;

[0047] (7) The molten steel is placed on the platform and allowed to stand for 15 to 30 minutes. The Als loss is controlled at 20 to 48 ppm when the RH is taken out of the station and sampled in the middle ladle (when the ladle is 1 / 2 filled).

[0048] (8) After the ingot is rolled, the results of the inclusion inspection of the ingot are shown in Table 2 below.

[0049] The control results of other parameters in the production process of each embodiment 1-6 and comparative examples 1-5 are shown in Table 2.

[0050] Table 2 Test results of various embodiments and comparative examples

[0051]

[0052] Table 2

[0053]

[0054] Table 2

[0055]

[0056] Table 2

[0057]

[0058] In Comparative Examples 3 and 4, less calcium wire is fed. Although it will not have a significant effect on the control of inclusions, it will affect the castability of the molten steel and the pouring rod position, which is also undesirable.

[0059] Practical application case 2:

[0060] Taking the production of 150t steel by converter smelting as an example, the specific production methods of each embodiment and comparative example are as follows:

[0061] (1) The steel produced in the embodiments and comparative examples is axle steel AAR M-101F. The main components of the molten steel in the tundish of each heat are shown in Table 3. The remainder not shown in Table 3 is Fe and unavoidable impurities.

[0062] Table 3 Molten steel composition (intermediate composition) of each heat / %

[0063]

[0064] (2) The P content of the molten iron entering the furnace is controlled at 0.11%~0.15%, the S content is controlled at 0.022%~0.036%, the iron-steel ratio is 15%~25%, and the scrap steel is low-sulfur scrap steel (the S content in the scrap steel is ≤0.015%);

[0065] (3) The C content at the end of the electric furnace is 0.08%~0.16%, the P content is 0.010%~0.013%, the [O] content at the end is 223~298ppm, the end temperature is 1632~1658℃, and the slag amount is about 2.4~3.7kg / ton of steel;

[0066] (4) When 1 / 3 of the steel is tapped, 3.5-4.5 kg / ton of aluminum iron, 2.5-4.0 kg / ton of lime, and 1.8-2.6 kg / ton of pre-melted refined slag are added in sequence; the pre-melted refined slag mainly has a CaO content of 45-55%, an Al2O3 content of 35-45%, a SiO2 content of ≤9%, a Mg content of ≤10%, and a particle size of 5-40 mm; during the tapping process, the ladle is strongly stirred (the bottom blowing argon gas flow rate is controlled at 500 NL / min);

[0067] (5) The composition of LF refining slag is CaO content 45~58%, SiO2 content 8~15%, Al2O3 content 23~35%, (FeO+MnO) is controlled at 0.2%~0.6%, binary basicity (CaO / SiO2) is controlled at 3.0~5.0, CaO / Al2O3 ratio is controlled at 1.3~2.0, the refining slag amount is controlled at 13~20kg / ton steel, the refining time after slag formation is 17~25min, and the LF refining cycle is controlled at 62~98min;

[0068] (6) Vacuum refining vacuum degree 59~86Pa, vacuum treatment cycle 15~20min, hydrogen [H] content 0.5~0.7ppm before breaking, Als and feed rate of vacuum process are shown in Table 4 below, 160~300kg of heat preservation agent is added during breaking, and soft blowing time is 15~25min;

[0069] (7) The molten steel is placed on the platform and allowed to stand for 15-29 minutes. The Als loss is controlled at 18-46 ppm when the RH is taken out of the station and sampled from the middle ladle (when the ladle is 1 / 2 cast).

[0070] (8) After the ingot is rolled, the results of the inclusion inspection of the shaft ingot are shown in Table 4 below.

[0071] The control results of other parameters in the production processes of Examples 7 to 13 and Comparative Examples 6 to 12 are shown in Table 4.

[0072] Table 4 Inclusion test results of various embodiments and comparative examples

[0073]

[0074] Table 4

[0075]

[0076] Table 4

[0077]

[0078] Table 4

[0079]

[0080] In Comparative Examples 7 and 8, less calcium wire is fed. Although it will not have a significant effect on the control of inclusions, it affects the castability of the molten steel and the pouring rod position is raised, which is also undesirable.

[0081] It can be seen from the embodiments and comparative examples that a high wire feeding amount will cause unstable control of inclusions, while a low wire feeding amount will result in poor improvement of the castability of molten steel. Only by establishing a relationship between vacuum Als loss and wire feeding amount according to the present invention can effective modification of inclusions be achieved, and stable casting rod position and inclusion stability control be achieved.

[0082] Comparison of inclusions in the casting and axle before and after the optimization process between Comparative Example 2 and Example 1 Figure 1-Figure 4 As shown, before optimization, the inclusions in the ingot are mainly point-like calcium aluminate and MnS inclusions, but there are a few large-sized calcium aluminate and individual clustered inclusions. After rolling, long strips, chains and spherical large-sized inclusions exist on the axle, and there is a risk in the inclusion rating. After optimization, the inclusions in the ingot are point-like calcium aluminate and MnS inclusions, and their sizes are relatively small. After rolling, the axle mainly contains blocky MnS and point-like calcium aluminate inclusions, and their sizes are relatively small. There is no inclusion rating and it is unqualified.

[0083] The underlined data in the table do not meet the requirements of the present invention.

[0084] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A method for controlling axle steel calcium treatment process, characterized in that: The axle steel calcium treatment process control method comprises the following steps: (1) For smelting, the molten iron entering the furnace must have a P content of ≤0.15% and a S content of ≤0.040%; (2) Deoxidation and alloying during the steel tapping process; (3) LF refining to adjust the composition of the refined slag; (4) Vacuum refining, after breaking the vacuum, feeding silicon calcium wire or pure calcium wire for calcium treatment; (5) After the molten steel is put on the stage and allowed to stand, pouring begins, and protective casting is used during the casting process; In step (4), the amount of silicon calcium wire or pure calcium wire fed is based on the aluminum loss Δ[Als] during the RH vacuum treatment process. RH Determine; feed amount L of calcium silicon wire Si-Ca线 =([20+1250×Δ[Als] RH ])×W s / 100±5m; or, feed the pure calcium wire with a wire feeding amount L Ca线 =([10+1875×Δ[Als] RH ])×W s / 100±5m; Δ[As] RH =[As 样① -As 样② ]×RH 真空 / (RH 真空 -3); Where Als 样① ①Als value of the sample before RH vacuum treatment, unit: %; Als 样② ②Als value of the sample 3 minutes before RH breaks, unit is %; RH 真空 is the RH vacuum treatment time, in min; Ws is the weight of molten steel, in t; L Si-Ca线 is the amount of calcium silicon wire fed, unit: m; L Ca线 is the feeding amount of pure calcium wire, unit is m; According to the axle steel calcium treatment process control method, the inclusion inspection pass rate of rolled axle steel billets reaches 100%, among which Class A coarse inclusions are all ≤1.0 level, Class B coarse inclusions are all ≤1.0 level, Class D coarse inclusions are all ≤1.5 level, and Class Ds inclusions are ≤1.0 level.

2. The axle steel calcium treatment process control method according to claim 1, characterized in that: In step (1), the endpoint control requirements of the converter or electric furnace are that the C content is 0.08% to 0.25%, the P content is ≤0.013%, and the [O] content is ≤300ppm; the endpoint temperature is 1600 to 1680°C, the slag blocking during steel tapping is strengthened, and the slag amount is controlled to be less than 4kg / ton of steel.

3. The axle steel calcium treatment process control method according to claim 1, characterized in that: In step (2), aluminum deoxidizer, slag material and alloy are added in sequence when 1 / 3 of the steel is tapped.

4. The axle steel calcium treatment process control method according to claim 3, characterized in that: In step (2), the slag-making material includes lime and pre-melted refined slag, wherein the amount of lime added is 2.5-4.5 kg / ton of steel, the amount of pre-melted refined slag added is 1.8-3.0 kg / ton of steel, and the target amount of alloy added is controlled according to the internal control lower limit of the steel grade; the pre-melted refined slag mainly consists of a CaO content of 45-55%, an Al2O3 content of 35-45%, a SiO2 content of ≤9%, a Mg content of ≤10%, and a particle size of 5-40 mm.

5. The axle steel calcium treatment process control method according to claim 1, characterized in that: In step (3), the refined slag composition control requirements are CaO content 40-60%, SiO2 content 8-18%, Al2O3 content 22-35%, (FeO+MnO)≤1.0%, binary basicity (CaO / SiO2) is controlled at 2.5-5.0, CaO / Al2O3 ratio is controlled at 1.0-2.0, the refined slag amount is controlled at 12-20kg / ton steel, the refining time after slag formation is ≥15min, and the LF refining cycle is controlled within 120min.

6. The axle steel calcium treatment process control method according to claim 1, characterized in that: In step (4), vacuum refining controls the vacuum degree to ≤100Pa, the vacuum treatment cycle is more than 15min, the hydrogen content before breaking the vacuum is ≤1.0ppm, and after breaking the vacuum, a wire feeding machine is used to feed silicon calcium wire or pure calcium wire for calcium treatment.

7. The axle steel calcium treatment process control method according to claim 1, characterized in that: In step (4), 150-350 kg of heat preservation agent is evenly added to the slag surface after calcium treatment. After the heat preservation agent is added, the molten steel is soft-blown, the bottom blowing flow rate is 10-50 NL / min, and the soft blowing time is 15-25 min.

8. The axle steel calcium treatment process control method according to claim 1, characterized in that: In step (5), after the molten steel is put on the stage, it is allowed to stand for 15 to 30 minutes before pouring. During the casting process, the long shroud of the large ladle + the middle ladle + the immersed shroud should be well protected, and the Als loss from the RH exit to the middle ladle sampling should be controlled within 50ppm.