An organic complex coated lithium manganate and its preparation method and application
By forming an organic complex coating layer on the surface of lithium manganate, the problem of manganese element dissolution in lithium manganate batteries is solved, the capacity and cycle performance of the battery are significantly improved, and the stability and life of the battery are enhanced.
Patent Information
- Application Number
- CN202410940668.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The dissolution phenomenon of manganese element in lithium manganate batteries leads to voltage and capacity attenuation. The existing technology cannot completely solve the manganese dissolution problem through niobium metal and aluminum isopropoxide coating methods.
The organic complex coating method is used to form an organic complex coating layer on the surface of lithium manganate, which prevents the reduction of manganese ions to the negative electrode through the complex reaction, thus improving the capacity and cycle performance of lithium manganate.
It effectively inhibits the dissolution of manganese ions, improves the battery capacity and cycle performance of lithium manganate, and enhances the energy density and cycle life of the battery.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ion batteries, and in particular to an organic complex-coated lithium manganate and a preparation method and application thereof. Background Art
[0002] Lithium manganese oxide battery is a lithium-ion battery that uses lithium manganese oxide (LiMn2O4) as the positive electrode material. As a positive electrode material, lithium manganese oxide has a high specific capacity and a low price, and can provide stable electrochemical performance. By optimizing the preparation process and structural design of the material, the electrochemical performance of the positive electrode material can be improved, and the energy density and cycle life of the battery can be enhanced. Therefore, it is widely used in electric vehicles, portable electronic devices, energy storage systems and other fields. However, lithium manganese oxide is prone to surface manganese dissolution in the battery system, causing serious problems of voltage and capacity attenuation.
[0003] In order to slow down the phenomenon of manganese dissolution in the positive electrode material of lithium-ion batteries, professionals in this field generally solve it in two aspects: coating and adding a complexing agent to the battery.
[0004] Among them, prior art 1: 202211076970.0 discloses a method for preparing lithium manganese oxide with strong stability. Niobium metal can replace part of the manganese position in lithium manganese oxide, thereby improving the cycle performance of lithium manganese oxide.
[0005] This solution forms a niobium metal coating on the surface of lithium manganese oxide after high-temperature calcination, thereby inhibiting the dissolution of manganese in lithium manganese oxide at high temperatures, while improving the conductivity and cycle performance.
[0006] Prior art 2: 202010445596.1 discloses a wet coating method for lithium manganate positive electrode material. The lithium manganate positive electrode material is prepared from LiCH3CO2·2H2O and Mn(CH3CO2)2·6H2O in a molar ratio of LiCH3CO2·2H2O:Mn(CH3CO2)2·6H2O=0.9-1.1:2, and then mixed with a complexing agent. After drying and calcining, polycrystalline and uniform LiMn2O4 powder is obtained; the complexing agent is aluminum isopropoxide.
[0007] This solution uses a wet coating method for lithium manganese oxide positive electrode materials to form an aluminum isopropoxide coating layer on the surface of lithium manganese oxide, thereby inhibiting the dissolution of manganese in lithium manganese oxide, greatly improving the quality of the lithium manganese oxide positive electrode material and enhancing the cycle performance.
[0008] It is not difficult to see that the above two schemes respectively use the method of adding niobium metal and aluminum isopropoxide wet coating to slow down the dissolution of manganese.
[0009] The problem that this scheme needs to solve: How to propose a new preparation method to reduce manganese dissolution. Summary of the invention
[0010] The purpose of the present invention is to provide a preparation method and application of organic complex-coated lithium manganate. The lithium manganate positive electrode material is coated on the surface of the lithium manganate by a wet method to form an organic complex coating agent layer. When manganese is dissolved in the lithium manganate, the organic complex coating agent will react with the dissolved manganese ions to complex them on the surface of the lithium manganate, preventing the manganese ions from being reduced to the negative electrode and precipitating, thereby improving the capacity and cycle performance of the lithium manganate.
[0011] To achieve the above object, the present application discloses a method for preparing organic complex-coated lithium manganate, comprising the following steps:
[0012] Step 1: Mixing and calcining a manganese source, a lithium source and a metal oxide to obtain a lithium manganate sintered material;
[0013] Step 2: crushing and sieving the lithium manganese oxide sintered material obtained in step 1 to obtain powder;
[0014] Step 3: mixing the powder obtained in step 2 with the organic complex coating agent solution, stirring, and evaporating to dryness to obtain organic complex coated lithium manganate;
[0015] The metal element in the metal oxide is selected from at least one of Nb, Mg, Co, V, Ti, Al, Zr, Zn and La, and in step 1, the ratio of the molar amount of manganese element in the manganese source to the molar amount of lithium element in the lithium source and the molar amount of the metal element in the metal oxide is 20-25:10-14:0.05-2;
[0016] In the step 3, the mass ratio of the powder to the organic complexing coating agent in the organic complexing coating agent solution is 1000-5000:1-50;
[0017] The organic complexing coating agent is selected from at least one of dodecylbenzene sulfonate, ethylenediaminetetraacetic acid, 1,2-cyclohexanebis-N-carboxymethylglycine, diethylenetriaminepentaacetic acid, ethylene glycol bis-α-aminoethyl ether tetraacetic acid, N-β-hydroxyethylethylenediaminetriacetic acid, ethylenediamine, and sulfosalicylic acid.
[0018] Preferably, in step 2, the median particle size of the powder is 8 to 12 um.
[0019] Preferably, the metal oxides are niobium pentoxide and titanium dioxide, and the molar ratio of the niobium element in the niobium pentoxide to the titanium element in the titanium dioxide is 0.8-1:0.8-1.
[0020] Preferably, the organic complexing coating agent is dodecylbenzene sulfonate and ethylenediaminetetraacetic acid, and the mass ratio of dodecylbenzene sulfonate to ethylenediaminetetraacetic acid is 0.8-1:1-1.2.
[0021] Preferably, the organic complex coating agent is a modified organic complex coating agent that has been alkalized.
[0022] Preferably, the specific preparation method of the modified organic complex coating agent after alkalization treatment is: mixing the organic complex coating agent and the alkaline substance in a molar ratio of 0.8-1:0.8-1 in water and alkalizing for 1-4 hours, wherein the alkaline substance is selected from at least one of lithium hydroxide, lithium carbonate, lithium bicarbonate and ammonia water.
[0023] Preferably, the calcination temperature of step 1 is 650° C. to 800° C., and the calcination time is 6 to 12 hours; and the stirring time of step 3 is 1 to 4 hours.
[0024] In addition, the present application also discloses an organic complex-coated lithium manganese oxide, which is prepared by the above-mentioned preparation method of the organic complex-coated lithium manganese oxide.
[0025] In addition, the present application also discloses a lithium-ion battery, comprising the above-mentioned organic complex-coated lithium manganese oxide as a positive electrode active material.
[0026] The beneficial effects of the present invention are:
[0027] The invention provides a preparation method and application of organic complex-coated lithium manganate. A lithium manganate positive electrode material is coated on the surface of the lithium manganate by a wet method to form an organic complex coating agent layer. When manganese dissolution occurs in the lithium manganate, the organic complex coating agent will undergo a complex reaction with the dissolved manganese ions, complexing them on the surface of the lithium manganate to prevent the manganese ions from being reduced to the negative electrode and precipitated, thereby improving the capacity and cycle performance of the lithium manganate. At the same time, metal doping is performed in the lithium manganate positive electrode material, and the manganese dissolution phenomenon is further suppressed by reducing the direct contact area between the electrolyte and the lithium manganate, thereby further improving the battery capacity and cycle performance. DETAILED DESCRIPTION
[0028] In the description of the present invention, it should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0029] Example 1
[0030] Step 1: Mix the manganese source, lithium source and niobium pentoxide in a high-speed mixer, and burn the mixture in a roller kiln at a temperature of 750°C for 8 hours. After the burning is completed, cool naturally to room temperature to obtain lithium manganate sintered material;
[0031] The molar ratio of manganese element in the manganese source, lithium element in the lithium source and niobium element in niobium pentoxide is 22:11.33:0.11.
[0032] Step 2: Crush and sieve the lithium manganate sintered material to obtain powder, and control the median particle size of the powder to be D50=10±2um.
[0033] Step 3: Mix the powder with sodium dodecylbenzene sulfonate in a mass ratio of 1000:1, stir for 3 hours, and evaporate to dryness to obtain organic complex-coated lithium manganate.
[0034] Example 2
[0035] The method is basically the same as Example 1, except that in step 1, a mixture of niobium pentoxide and titanium dioxide is used to react with niobium pentoxide while the total molar amount of the metal element remains unchanged, and the molar ratio of niobium element in niobium pentoxide to titanium element in titanium dioxide is 0.9:0.9.
[0036] Example 3
[0037] The method is basically the same as Example 1, except that in step 3, a mixture of sodium dodecylbenzene sulfonate and ethylenediaminetetraacetic acid is used while the total molar amount of the organic complexing coating agent remains unchanged, and the mass ratio of sodium dodecylbenzene sulfonate to ethylenediaminetetraacetic acid is 0.9:1.1.
[0038] Example 4
[0039] The method is basically the same as Example 1, except that in step 1, a mixture of niobium pentoxide and titanium dioxide is used to react with niobium pentoxide while the total molar amount of the metal element remains unchanged, and the molar ratio of niobium element in niobium pentoxide to titanium element in titanium dioxide is 1:0.8.
[0040] Example 5
[0041] The method is basically the same as Example 1, except that in step 1, a mixture of niobium pentoxide and titanium dioxide is used to react with niobium pentoxide while the total molar amount of the metal element remains unchanged, and the molar ratio of the niobium element in the niobium pentoxide to the titanium element in the titanium dioxide is 0.8:1.
[0042] Example 6
[0043] The method is basically the same as Example 1, except that in step 3, the organic complexing coating agent is sodium dodecylbenzene sulfonate and ethylenediaminetetraacetic acid, and the mass ratio of sodium dodecylbenzene sulfonate to ethylenediaminetetraacetic acid is 1:1.
[0044] Example 7
[0045] The method is basically the same as Example 1, except that in step 3, calcium dodecylbenzenesulfonate and ethylenediaminetetraacetic acid are selected as the organic complexing coating agent, and the mass ratio of calcium dodecylbenzenesulfonate to ethylenediaminetetraacetic acid is 0.8:1.2.
[0046] Example 8
[0047] The method is basically the same as Example 2, except that in step 3, the organic complexing coating agent is a mixture of potassium dodecylbenzenesulfonate and ethylenediaminetetraacetic acid, and the mass ratio of potassium dodecylbenzenesulfonate to ethylenediaminetetraacetic acid is 0.9:1.1.
[0048] Example 9
[0049] The method is basically the same as Example 1, except that in step 1, the molar ratio of manganese element in the manganese source, lithium element in the lithium source and niobium element in niobium pentoxide is 20:10:0.05, the calcination temperature is 650° C., and the calcination time is 6 hours;
[0050] In step 3, the mass ratio of the powder to the organic complex coating agent sodium dodecylbenzene sulfonate is 1000:1, and the stirring time is 1 hour.
[0051] Example 10
[0052] The method is basically the same as Example 1, except that in step 1, the molar ratio of manganese element in the manganese source, lithium element in the lithium source and niobium element in niobium pentoxide is 25:13.75:2, the calcination temperature is 800° C., and the calcination time is 12 h.
[0053] In step 3, the mass ratio of powder to sodium dodecylbenzene sulfonate is 100:1, and the stirring time is 4 hours.
[0054] Embodiment 11
[0055] It is basically the same as Example 8, except that, during the sintering process of step 1, the sintering temperature is 550° C. and the sintering time is 8 hours.
[0056] Example 12
[0057] The method is basically the same as Example 1, except that in step 3, sodium dodecylbenzene sulfonate and lithium carbonate are mixed in water at a molar ratio of 1:1, alkalized for 2.5 hours, and modified sodium dodecylbenzene sulfonate is obtained; the powder is mixed with the modified sodium dodecylbenzene sulfonate at a mass ratio of 1000:1, stirred for 3 hours, and evaporated to obtain organic complex-coated lithium manganate.
[0058] Comparative Example 1
[0059] Step 1: Mix the manganese source and lithium source in a high-speed mixer at a molar ratio of 22:11.33, and burn the mixture in a roller kiln at a temperature of 750°C for 8 hours. After the burning, cool naturally to room temperature to obtain lithium manganate sintered material.
[0060] Step 2: Crush and sieve the lithium manganate sintered material, control the median particle size at D50=8~12um, and obtain the lithium manganate material.
[0061] Comparative Example 2
[0062] It is basically the same as Comparative Example 1, except that in step 1, the molar ratio of the manganese source, the lithium source and the niobium pentoxide is 22:11.33:0.11.
[0063] Comparative Example 3
[0064] It is basically the same as Comparative Example 1, except that:
[0065] Step 3: Mix the powder and sodium dodecylbenzene sulfonate in a mass ratio of 1000:1, stir, and evaporate to dryness to obtain a lithium manganese oxide material.
[0066] Full electrical performance test
[0067] The obtained lithium manganate is mixed evenly with 97% by mass, 1.5% PVDF and 1.5% carbon nanotubes to prepare a slurry for coating. The steps are as follows:
[0068] 1. Dissolve PVDF in NMP to prepare a glue solution with a solid content of 8%, then add carbon nanotube slurry and mix and disperse at high speed for 1.5 hours, then add this product and knead and stir for 6 hours, add an appropriate amount of NMP to adjust the slurry viscosity to 4500-7500mPa.s. Obtain positive electrode slurry for lithium batteries.
[0069] 2. A negative electrode slurry is prepared by a similar method and formula to obtain a negative electrode slurry for lithium battery.
[0070] 3. The positive electrode slurry is coated on the aluminum foil, and the negative electrode slurry is coated on the copper foil. After drying, rolling, powder stripping, welding of pole ears, winding, liquid injection, sealing and other processes, the soft pack battery is prepared, and the battery capacity, cycle and short circuit experiments are tested. The experimental results are shown in Table 1:
[0071] Table 1
[0072] experiment Median particle size / um Full battery capacity / mAh / g Cycle life (weeks) Storage at 60℃ for 7 days: remaining capacity (%) Capacity recovery rate after 7-day storage at 60℃ (%) Example 1 11.0 118.0 490 82.0 93.4 Example 2 11.3 119.0 520 83.4 94.5 Example 3 10.5 119.3 523 83.8 94.6 Example 4 11.6 118.6 513 83.2 93.4 Example 5 11.8 119.0 515 82.4 93.4 Example 6 10.5 118.2 515 83.6 94.0 Example 7 11.0 117.5 510 82.0 93.4 Example 8 11.0 123 560 86.0 95.6 Example 9 11.8 118 480 81.9 93.3 Example 10 10.6 110 488 81.8 93.0 Embodiment 11 11.0 118.2 495 83 94.0 Example 12 10.8 119.5 525 83.7 94.4 Comparative Example 1 11.0 115.0 150 30 36 Comparative Example 2 10.5 115.3 200 45 55 Comparative Example 3 11.2 116.5 350 65 77
[0073] Result analysis:
[0074] 1. It can be seen from Examples 1-3 that, in the present invention, the combined use of metal oxides or organic complex coating agents can improve the cycle performance and storage performance of the battery, and the cycle performance is significantly improved.
[0075] 2. It can be seen from Examples 1-2 and 4-5 that in the present invention, when the metal compound is a mixture of niobium pentoxide and titanium dioxide, the performance of the battery can be effectively improved, and the optimal molar ratio of niobium element to titanium element is 0.9:0.9.
[0076] 3. It can be seen from Examples 1, 3 and 6-7 that in the present invention, when the organic complex coating agent is a mixture of dodecylbenzene sulfonate and ethylenediaminetetraacetic acid, the manganese ions dissolved from lithium manganate can be effectively complexed on the surface of the lithium manganate, preventing the manganese ions from being reduced to the negative electrode and precipitated, thereby improving the capacity, cycle performance and storage performance of the lithium manganate; and when the mass ratio of dodecylbenzene sulfonate to ethylenediaminetetraacetic acid is 0.9:1.1, the effect is best.
[0077] 4. It can be seen from Examples 1-3 and Example 8 that in the present invention, the effect of using the metal oxide or the organic complex coating agent alone or using the metal oxide or the organic complex coating agent together after being compounded compared with Example 1 on improving the battery performance is shown in Table 2 below:
[0078] Improvement rate = (A-Example 1) / Example 1×100, A is the value of Example 2, Example 3, and Example 8;
[0079] Table 2
[0080] experiment Full battery capacity improvement rate (%) Cycle life (weeks) improvement rate (%) Storage at 60℃ for 7 days: Remaining capacity increase rate (%) Capacity recovery rate after 7-day storage at 60°C (%) Example 2 0.85 6.12 1.71 1.18 Example 3 1.10 6.73 2.20 1.28 Example 8 4.24 14.29 4.88 2.36
[0081] It can be seen from Table 2 that when the metal oxide compound and the organic complex coating agent compound work together, the synergistic effect of the two makes the improvement effect on battery performance greater than the improvement effect of the metal oxide or the organic complex coating agent used alone. Therefore, the mixture of niobium pentoxide and titanium dioxide with a molar ratio of niobium to titanium of 0.9:0.9 and the mixture of dodecylbenzene sulfonate and ethylenediaminetetraacetic acid with a mass ratio of dodecylbenzene sulfonate to ethylenediaminetetraacetic acid of 0.9:1.1 are the best ratios.
[0082] 5. It can be seen from Example 1 and Comparative Examples 1-3 that in the present invention, the use of metal oxide or organic complex coating agent alone and the combination of the two have an improvement effect on battery performance compared with Comparative Example 1 as shown in Table 3:
[0083] Improvement rate = (B-Comparative Example 1) / Comparative Example 1×100, B is the value of Comparative Example 2, Comparative Example 3, and Example 1;
[0084] Table 3
[0085] experiment Full battery capacity improvement rate (%) Cycle life (weeks) improvement rate (%) Storage at 60℃ for 7 days: Remaining capacity increase rate (%) Capacity recovery rate after 7-day storage at 60°C (%) Comparative Example 2 0.52 33.33 50.00 52.78 Comparative Example 3 1.30 133.33 116.67 113.89 Example 1 2.61 226.67 173.33 159.44
[0086] It can be seen from Table 3 that the effect of using a combination of metal oxide and an organic complex coating agent on improving battery performance is greater than the effect of using either metal oxide or organic complex coating agent alone.
[0087] 6. It can be seen from Example 1 and Example 12 that in the present invention, when the organic complex coating agent and the alkaline substance are alkalized and modified, the various performances of the battery can be better improved.
[0088] 7. Observe Table 4, through Example 1, Example 8 and Example 11, it can be seen that in the present invention, both Example 8 and Example 11 improve the battery performance, but the mechanism of action is different. Example 11 is doping metal elements, while Example 8 is coating metal elements; coating metal elements is through high-temperature sintering, so that the metal migrates outward during the sintering process to form a coating layer. And from the data in Table 4, it can be seen that the improvement effect of coating metal elements is better than that of doping metal elements.
[0089] Table 4
[0090] experiment Median particle size / um Full battery capacity / mAh / g Cycle life (weeks) Storage at 60℃ for 7 days: remaining capacity (%) Capacity recovery rate after 7-day storage at 60℃ (%) Example 1 11.0 118.0 490 82.0 93.4 Example 8 11.0 123 560 86.0 95.6 Embodiment 11 11.0 118.2 495 83 94.0
[0091] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. A method for preparing organic complex-coated lithium manganate, characterized in that: The steps include: Step 1: Mixing and calcining a manganese source, a lithium source and a metal oxide to obtain a lithium manganate sintered material; Step 2: crushing and sieving the lithium manganese oxide sintered material obtained in step 1 to obtain powder; Step 3: mixing the powder obtained in step 2 with the organic complex coating agent solution, stirring, and evaporating to dryness to obtain organic complex coated lithium manganate; In the step 1, the ratio of the molar amount of manganese element in the manganese source to the molar amount of lithium element in the lithium source and the molar amount of metal element in the metal oxide is 20-25:10-14:0.05-2; In the step 3, the mass ratio of the powder to the organic complexing coating agent in the organic complexing coating agent solution is 1000-5000:1-50; The metal oxides are niobium pentoxide and titanium dioxide, and the molar ratio of the niobium element in the niobium pentoxide to the titanium element in the titanium dioxide is 0.8-1:0.8-1; The organic complexing coating agent is dodecylbenzene sulfonate and ethylenediaminetetraacetic acid, and the mass ratio of dodecylbenzene sulfonate to ethylenediaminetetraacetic acid is 0.8-1:1-1.
2.
2. The method for preparing organic complex coated lithium manganate according to claim 1, characterized in that: In step 2, the median particle size of the powder is 8 to 12 um.
3. The method for preparing organic complex coated lithium manganate according to claim 1, characterized in that: The organic complex coating agent is a modified organic complex coating agent that has been alkalized.
4. The method for preparing organic complex coated lithium manganate according to claim 3, characterized in that: The specific preparation method of the modified organic complex coating agent after alkalization treatment is: mixing the organic complex coating agent and the alkaline substance in a molar ratio of 0.8-1:0.8-1 in water and alkalizing for 1-4 hours, wherein the alkaline substance is selected from at least one of lithium hydroxide, lithium carbonate, lithium bicarbonate and ammonia water.
5. The method for preparing organic complex coated lithium manganate according to claim 1, characterized in that: The calcination temperature of step 1 is 650° C. to 800° C., and the calcination time is 6 to 12 hours; the stirring time of step 3 is 1 to 4 hours.
6. An organic complex coated lithium manganate, characterized in that: The method is prepared by the method for preparing organic complex-coated lithium manganate according to any one of claims 1 to 5.
7. A lithium ion battery, characterized in that: A positive electrode comprising the organic complex-coated lithium manganate as claimed in claim 6 as an active material.
Citation Information
Patent Citations
Lithium manganate cathode material wet coating method
CN111640922A
Preparation method of high-stability lithium manganate
CN115465896A
One-step doped, coated and modified NCM ternary positive electrode material and preparation method thereof
CN113506874A
Lithium-rich manganese-based precursor, positive electrode material, lithium ion battery and preparation method of lithium-rich manganese-based precursor
CN116040699A
Spinel-type lithium manganate and method for producing the same and use of the same
JP2023162089A