A method for preparing nano-scale hydrotalcite based on microreactor

By performing countercurrent mass transfer reaction and microwave heating in a micro reactor, combined with full mixing of carbon dioxide and air, the problem of uneven particle size of nano-scale aluminum magnesium carbonate in industrial production was successfully solved, and a stable and efficient nano-scale was achieved Magnesium aluminum carbonate preparation, suitable for industrial production.

CN118495571BActive Publication Date: 2024-10-01JINAN TONGLU PHARM TECH & DEV CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410646719.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-10-01
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

It is difficult for the prior art to effectively prepare nano-scale magnesium aluminum carbonate in industrial production. Conventional methods have problems of uneven particle size and poor fluidity, resulting in poor chewing taste of oral tablets and poor dispersion of suspension preparations.

Method used

The preparation of nanoscale magnesium aluminum carbonate is carried out by using a micro reactor. By mixing alkaline reagents with water-soluble aluminum salts and magnesium salts in the micro reactor, and heating them with microwave generator components to reduce the reaction activation energy. , the reaction rate is increased, and then thoroughly mixed with carbon dioxide and air, and the pH value is controlled to obtain nanoscale magnesium aluminum carbonate.

Benefits of technology

It has achieved stable preparation of nano-grade magnesium aluminum carbonate, with a particle size of about 200nm, which is suitable for industrial production, and does not require high-temperature crushing, good stability, and avoids the limitation of the grinding effect by factors such as equipment speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495571B_ABST
    Figure CN118495571B_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of nano-scale aluminum carbonate based on a microreactor. In the method, an alkaline solution and a salt solution are prepared by using an alkaline reagent, a water-soluble aluminum salt and a water-soluble magnesium salt. After the dispersed phase alkali solution is dispersed into small particles through micropores of micrometer level inside the microreactor, it reacts with a mobile phase salt solution in a reaction tube of the microreactor to obtain small-particle-size insoluble magnesium and aluminum hydroxide, that is, a mixed solution. A mixed gas of carbon dioxide and air is used as a dispersed phase, and after the dispersed phase is dispersed through micropores of micrometer level inside the microreactor, it reacts with an insoluble slurry of the mobile phase in the reaction tube of the microreactor to obtain a nano-scale reaction solution. After filtering, washing and drying, the nano-scale reaction solution obtains a nano-scale aluminum carbonate having a particle size of about 200nm of D90, and the quality is stable. The microreactor and production system used in the preparation process of aluminum carbonate do not require high temperature, crushing, or amplification effect, have good stability, and are suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of synthetic pharmaceuticals and relates to a preparation method of nano-scale hydrotalcite based on a microreactor. Background Art

[0002] Magnesium aluminum carbonate has a molecular weight of 603.98 and a molecular formula of Al2Mg6(OH)16CO3·4H2O. It is a white or off-white granular powder that is insoluble in water but soluble in hydrochloric acid to produce bubbles. Magnesium aluminum carbonate, as a new type of antacid, can react quickly with acid to improve or relieve various symptoms caused by excessive gastric acid.

[0003] The conventional preparation method of hydrotalcite mainly relies on autoclave reaction crystallization, which has the problems of large average particle size, wide particle size distribution, and poor fluidity. The particle size problem will lead to poor chewing taste of oral tablets and poor dispersibility of suspension preparations. At present, the nano-scale hydrotalcite used by relevant domestic units mainly relies on imports.

[0004] The patent with publication number CN101381094A discloses a method for preparing nano magnesium aluminum hydrotalcite, which comprises: preparing a magnesium and aluminum mixed salt solution and an ammonium bicarbonate solution; adding the two mixed solutions simultaneously into a static mixer to undergo a chemical reaction; and then passing through a aging reactor to allow the magnesium aluminum hydrotalcite microcrystals to grow to obtain a nano magnesium aluminum hydrotalcite product. The particle size of the prepared nano magnesium aluminum hydrotalcite product is not specified.

[0005] The patent publication number CN106379924A discloses a method for preparing nano magnesium aluminum hydrotalcite, which uses magnesium chloride, aluminum chloride, sodium carbonate and sodium hydroxide as main raw materials, adds sodium oleate as a foaming aid, first prepares a precursor filter cake by bubble liquid film reaction, then undergoes hydrothermal reaction, filtration, washing and drying. The D50 of the prepared magnesium aluminum hydrotalcite is below 3 μm.

[0006] Patent publication number CN116102046A discloses a method for crystallizing hydrotalcite with narrow particle size distribution in micrometers, which uses magnesium chloride, aluminum chloride, sodium carbonate and sodium hydroxide as main raw materials, controls the particle size distribution by ultrasonic equipment during the hydrothermal reaction, and then obtains hydrotalcite by filtering, washing and drying. The D50 of the prepared hydrotalcite is above 10 μm.

[0007] The patent with publication number CN112274532A discloses a nano-aluminum carbonate crystal suspension and a preparation method thereof, wherein the method adopts wet grinding, sodium hexametaphosphate as a dispersant, and the particle size of the aluminum carbonate is controlled by adjusting the rotation speed, grinding medium, and grinding time of the grinder, and aluminum carbonate nano-crystalline particles in the suspension are obtained by long-term grinding. The prepared aluminum carbonate nano-crystalline particles have a D90 of 352nm, a D50 of 161nm, and a D10 of 76nm.

[0008] The particle size of the hydrotalcite prepared in the above patents does not reach the nanometer level except for the patent with publication number CN112274532A. Although the patent with publication number CN112274532A can control the particle size of hydrotalcite to the nanometer level through the grinding method, the grinding equipment involved in the preparation process only stays at the laboratory level. At the same time, after the grinding equipment is enlarged, it is limited by factors such as the rotation speed of the equipment, and the grinding effect will be greatly reduced, which makes it difficult to industrialize the production of nano-scale hydrotalcite. Summary of the invention

[0009] The purpose of the present invention is to provide a method for preparing nano-scale hydrotalcite based on a microreactor, so as to solve the problem of difficulty in the industrial production of existing nano-scale hydrotalcite.

[0010] To achieve the above object, the present invention adopts the following technical solutions:

[0011] The present invention provides a method for preparing nano-scale hydrotalcite based on a microreactor, the method comprising:

[0012] S01: Add alkaline reagent into purified water, stir to dissolve, filter, and obtain alkaline solution.

[0013] Add an alkaline agent to 10-12 parts of purified water, stir to dissolve, and filter to obtain a filtrate as an alkaline solution. In the present application, the alkaline agent includes sodium hydroxide or potassium hydroxide; preferably, the alkaline agent is sodium hydroxide.

[0014] S02: Add water-soluble aluminum salt and water-soluble magnesium salt into purified water, stir to dissolve, filter, and obtain a salt solution.

[0015] A water-soluble aluminum salt and a water-soluble magnesium salt are added to 10-12 parts of purified water, stirred to dissolve, and filtered to obtain a filtrate as a saline solution. In the present application, the water-soluble aluminum salt includes aluminum chloride, aluminum sulfate or aluminum nitrate, and the water-soluble magnesium salt includes magnesium sulfate or magnesium chloride. Preferably, the water-soluble aluminum salt is aluminum chloride, and the water-soluble magnesium salt is magnesium chloride.

[0016] S03: The salt solution is used as a mobile phase to enter the reaction tube of the microreactor, and the alkali solution is used as a dispersed phase to enter the interior of the reactor body of the microreactor, and then enters the reaction tube through the micropores on the side wall of the reactor body. The salt solution and the alkali solution are mixed and reacted in a countercurrent mass transfer manner in the reaction tube to obtain a mixed solution.

[0017] With saline as the mobile phase and alkali as the dispersed phase, the saline and alkali are introduced into the reaction tube and the reactor body of the microreactor respectively under the conditions of a feed flow rate ratio of 1:1 and a feed concentration molar ratio of 1: (2.75-3.5). The alkali enters the reaction tube after being dispersed through the micropores at the micron level on the side wall of the reactor body. The saline and the small-particle alkali dispersed by the micropores are fully mixed in the annular reaction tube, which greatly increases the counter-current mass transfer effect of the two phases. At the same time, the microwave generator assembly inside the microreactor can achieve internal integrity, rapid heating and non-thermal effects, thereby reducing the reaction activation energy and accelerating the reaction rate. In this way, the saline and alkali react in a counter-current mass transfer mixture in the reaction tube of the microreactor, and the reaction is accelerated rapidly from the aspects of mass transfer, heat transfer and microwave reduction of the reaction activation energy, and small-particle insoluble magnesium and aluminum hydroxides are obtained, which is the mixed solution.

[0018] In the present application, the molar ratio of the water-soluble aluminum salt, the water-soluble magnesium salt and the alkaline agent is 1:3:(11-14). Preferably, the molar ratio of the water-soluble aluminum salt, the water-soluble magnesium salt and the alkaline agent is 1:3:12.

[0019] In the present application, the microreactor comprises a reactor body, a reaction tube and a microwave generator assembly which are sealed in sequence from the outside to the inside, wherein micropores are provided on the tube wall of the reaction tube; after the dispersed phase entering the reactor body passes through the micropores, it reacts with the mobile phase in a countercurrent mass transfer in the cavity between the reaction tube and the microwave generator assembly.

[0020] In the present application, the angle between the opening direction of the micropore and the flow direction of the mobile phase is 0-90°, and the diameter of the micropore is 1-2000 μm.

[0021] In the present application, the microwave generator assembly includes a microwave-transparent generator sleeve, a microwave generator clamped on the inner wall of the generator sleeve, and a microwave controller electrically connected to the microwave generator; the generator sleeve is fixed to the inner wall of the reaction tube by a supporting foot, and the microwave controller is located outside the reactor body.

[0022] S04: The mixed solution is stirred and mixed with a water-soluble dispersant to obtain an insoluble slurry.

[0023] After the microreactor reaction is completed, the mixed solution is transferred to a reactor containing a water-soluble dispersant, stirred and mixed to obtain a slurry containing insoluble magnesium and aluminum hydroxide, that is, an insoluble slurry. In the present application, the water-soluble dispersant includes polyethylene glycol, polyvinyl alcohol, cellulose acetate or polyvinyl pyrrolidone, and its amount is 1-5% of the total water consumption. Preferably, the water-soluble dispersant is polyethylene glycol, and its amount is 2% of the total water consumption.

[0024] S05: The insoluble slurry is used as a mobile phase to enter the reaction tube of the microreactor, and the mixed gas of carbon dioxide and air is used as a dispersed phase to enter the reactor body of the microreactor, and then enters the reaction tube through the micropores on the side wall of the reactor body. The insoluble slurry and the mixed gas are mixed and reacted in a countercurrent mass flow in the reaction tube. When the pH value of the material reaches 10-12 during the mixed reaction, the reaction is stopped to obtain a reaction solution.

[0025] With an insoluble slurry as the mobile phase and a mixture of carbon dioxide and air as the dispersed phase, the insoluble slurry and the mixed gas are respectively introduced into the reaction tube and the reactor body of the microreactor at a feed flow rate ratio of 1: (1.1-1.5). The mixed gas enters the reaction tube after being dispersed through micropores at the micron level on the side wall of the reactor body. The insoluble slurry and the mixed gas dispersed by the micropores are fully mixed in the annular reaction tube, which increases the countercurrent mass transfer effect of the two phases. At the same time, the microwave generator assembly inside the microreactor can achieve internal overall and rapid heating without external heating, promoting the reaction of the insoluble slurry with carbon dioxide in the mixed gas. When the pH value of the material reaches 10-12 during the mixed reaction, the reaction is stopped to obtain a nanoscale reaction liquid.

[0026] In the present application, the concentration of carbon dioxide in the mixed gas is 10-30%. Preferably, the concentration of carbon dioxide in the mixed gas is 15%, and the pH value of the material during the mixed reaction is 10-11.

[0027] S06: The reaction solution is filtered, washed and dried to obtain nano-scale hydrotalcite.

[0028] The filter cake obtained by filtering the reaction solution is washed with purified water and then dried at a temperature of 70-80° C. for 20-22 hours to obtain nano-scale aluminum carbonate.

[0029] The present invention has the following beneficial effects:

[0030] (1) Alkaline solution and salt solution are prepared with alkaline reagent, water-soluble aluminum salt and water-soluble magnesium salt. The salt solution is used as the mobile phase and the alkaline solution is used as the dispersed phase, which are respectively introduced into the reaction tube and the reactor body of the microreactor. After the alkaline solution is dispersed into small particles through the micropores on the side wall of the reactor body at the micron level, it is mixed and reacted with the salt solution in the reaction tube in a countercurrent mass transfer, and the reaction is accelerated from multiple aspects such as mass transfer, heat transfer and microwave reduction of the reaction activation energy, thereby obtaining small-particle insoluble magnesium and aluminum hydroxides, which is the mixed solution.

[0031] (2) After the mixed liquid and the water-soluble dispersant are stirred and mixed into an insoluble slurry, the insoluble slurry is used as the mobile phase and the mixed gas of carbon dioxide and air is used as the dispersed phase, which are introduced into the reaction tube and the reactor body of the microreactor respectively. The mixed gas is dispersed through the micropores at the micrometer level on the side wall of the reactor body and then enters the reaction tube, where it is fully mixed with the insoluble slurry in the annular reaction tube, thereby increasing the countercurrent mass transfer effect of the two phases. At the same time, the microwave generator assembly inside the microreactor can achieve internal overall and rapid heating without the need for external heating. The insoluble slurry reacts with the carbon dioxide in the mixed gas at room temperature to obtain a nanoscale reaction liquid.

[0032] (3) The particle size D90 of the nano-scale aluminum carbonate magnesium prepared in the present application is about 200 nm, and the quality is stable.

[0033] (4) The microreactor and nano-scale aluminum carbonate magnesium production system does not require high temperature, crushing, or amplification effect, has good stability, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a schematic diagram of the process for preparing nano-scale aluminum carbonate in the embodiment of the present application;

[0035] Figure 2 This is a schematic diagram of the structure of a microreactor in an embodiment of the present application;

[0036] Figure 3 This is a particle size distribution diagram of the hydrotalcite prepared in Example 1 of the present application;

[0037] Figure 4 This is a particle size distribution diagram of the hydrotalcite prepared in Comparative Example 1 of the present application;

[0038] Figure 5 This is a particle size distribution diagram of the hydrotalcite prepared in Comparative Example 2 of the present application;

[0039] Figure 6 This is a particle size distribution diagram of the hydrotalcite prepared in Comparative Example 3 of the present application;

[0040] Symbols represent:

[0041] 1-reactor body, 2-reaction tube, 3-microwave generator assembly, 4-micropore, 5-support foot, 6-mobile phase feed port, 7-discharge port, 8-dispersed phase feed port, 9-dispersion chamber, 10-mixing reaction chamber;

[0042] 301-generator casing, 302-microwave generator, 303-microwave controller. DETAILED DESCRIPTION

[0043] The technical solution of the present invention is further explained and illustrated by means of specific embodiments below.

[0044] Attached Figure 1 The preparation flow chart of nano-scale hydrotalcite based on microreactor is shown. Figure 1 It can be seen that in the preparation method of nano-scale hydrotalcite based on microreactor provided in the embodiment of the present application, alkali solution is prepared with alkaline reagent, and pumped into microreactor after valve and centrifugal pump. Salt solution is prepared with water-soluble aluminum salt and water-soluble magnesium salt, and pumped into microreactor after valve and centrifugal pump. After the dispersed phase alkali solution is dispersed into small particle size by micropores of micron level inside microreactor, it reacts with mobile phase salt solution in the reaction tube of microreactor to obtain small particle size insoluble magnesium and aluminum hydroxide, i.e., mixed solution. With the mixed gas of carbon dioxide and air as dispersed phase, the dispersed phase is dispersed by micropores of micron level inside microreactor and reacts with mobile phase insoluble slurry in the reaction tube of microreactor to obtain nano-scale reaction solution. The nano-scale reaction solution obtains nano-scale hydrotalcite after filtration, washing and drying.

[0045] The microreactor in the embodiment of the present application includes a reactor body 1, a reaction tube 2 and a microwave generator assembly 3 which are sequentially sealed from the outside to the inside. Figure 2 shown.

[0046] Specifically, a dispersed phase feed port 8 is provided on the side wall of the reactor body 1, so that the dispersed phase material can enter the interior of the reactor body 1 through the dispersed phase feed port 8 to achieve material dispersion. The dispersed phase material in the embodiment of the present application is a mixture of alkali solution or carbon dioxide and air. A mobile phase feed port 6 is provided at the bottom of the reaction tube 2, and the mobile phase material enters the interior of the reaction tube 2 through the mobile phase feed port 6 at the bottom. The mobile phase material in the embodiment of the present application is a saline solution or an insoluble slurry. A discharge port 7 is also provided at the top of the reaction tube 2 for discharging the reaction product obtained after the dispersed phase material and the mobile phase material react. The length of the discharge port 7 can be freely adjusted, and the material can be discharged quickly to achieve continuous production.

[0047] In the embodiment of the present application, the cavity between the reactor body 1 and the reaction tube 2 forms a dispersion cavity 9, which is mainly used for dispersing the dispersed phase material. The cavity between the reaction tube 2 and the microwave generator assembly 3 forms a mixing reaction cavity 10, which is mainly used for rapid contact and full mixing of the dispersed phase material and the mobile phase material to accelerate the reaction.

[0048] The wall of the reaction tube 2 is provided with many tiny micropores 4. The dispersed phase material in the dispersion chamber 9 enters the reaction tube 2 through the micropores 4, and then quickly contacts with the mobile phase material in the mixing reaction chamber 10, and then is fully mixed and counter-flows. In order to prevent the micropores 4 from being blocked, it is necessary to adjust the pressure of the dispersed phase material to be higher than the pressure of the mobile phase material, so that the dispersed phase material can open the micropores 4 at a higher pressure.

[0049] In order to make the dispersed phase material and the mobile phase material fully contact in countercurrent and increase the mass transfer effect, in the embodiment of the present application, the angle α between the opening direction of the micropore 4 and the flow direction of the mobile phase is 0-90°. In addition, in the embodiment of the present application, the diameter of the micropore 4 is 1-2000 μm, and the diameter of the micropore 4 needs to be specifically selected according to the viscosity of the dispersed phase, the pressure of the delivery pump, and the requirements of mixed mass transfer.

[0050] In the embodiment of the present application, the microwave generator assembly 3 includes a generator sleeve 301, a microwave generator 302 and a microwave controller 303. The generator sleeve 301 is fixed to the inner wall of the reaction tube 2 by a plurality of support feet 5. A slot (not shown in the figure) is provided on the inner wall of the generator sleeve 301, and the microwave generator 302 is snapped into the slot of the generator sleeve 301 to fix the microwave generator 302. The microwave controller 303 is arranged outside the reactor body 1 and is electrically connected to the microwave generator 302.

[0051] The generator sleeve 301 can not only isolate the microwave generator 302 from the reaction materials, but also has good microwave penetration, so that the microwaves generated by the microwave generator 302 can directly act on the reaction materials after passing through the generator sleeve 301. Since the generator sleeve 301 is arranged in the reaction tube 2 and the generator sleeve 301 is cylindrical, the mixing reaction chamber 10 forms a ring structure accordingly, which is conducive to the full mixing of the dispersed phase material and the mobile phase material, thereby facilitating the reaction.

[0052] The microwave generator 302 is the core component of the microwave generator assembly 3, which can convert direct current power into microwave energy to generate microwaves. The generation of microwaves can generate a thermal effect inside the molecules of the dispersed phase material and the mobile phase material after uniform mixing, greatly accelerating the chemical reaction rate and shortening the reaction time. The core component of the microwave generator 302 is a microwave tube. In order to facilitate the rapid contact microreactor provided in the embodiment of the present application to be in a continuous working state, the microwave tube in the embodiment of the present application uses a continuous wave magnetron.

[0053] The microwave controller 303 can convert AC power into DC power, which makes it easier for the microwave generator 302 to convert the DC power generated by the microwave controller 303 into microwave energy, thus providing working conditions for the microwave generator 302. At the same time, the microwave controller 303 can also adjust and control the microwave frequency through the conversion of power to adapt to different chemical reactions.

[0054] The following is a detailed description of the preparation method of nano-scale aluminum carbonate magnesium based on a microreactor provided in the embodiment of the present application and the preparation method provided in the comparative example in the form of specific examples combined with drawings.

[0055] Example 1

[0056] The present application embodiment provides a method for preparing nano-scale hydrotalcite based on a microreactor, the method comprising:

[0057] S101: Add 9.60 kg of sodium hydroxide to 96 kg of purified water, stir to dissolve, and filter into a measuring kettle. The volume of the filtrate obtained by filtration is supplemented to 110 L to obtain an alkali solution with a concentration of 2.18 mol / L.

[0058] S102: Add 2.67 kg aluminum chloride and 5.71 kg magnesium chloride to 85 kg purified water, stir to dissolve, filter to a measuring kettle, and add the volume of the filtrate to 110 L to obtain a salt solution with a concentration of 0.73 mol / L.

[0059] S103: With saline as the mobile phase, it enters the reaction tube of the microreactor at a feed flow rate of 3L / min. With alkali solution as the dispersed phase, it enters the reactor body of the microreactor at a feed flow rate of 3L / min, and then enters the reaction tube after being dispersed through the micropores of micrometer level on the side wall of the reactor body. The saline solution and the small-particle alkali solution dispersed by the micropores are fully mixed in the annular reaction tube, and the microwave generator assembly inside the microreactor is turned on to react to obtain a mixed solution. Among them, the molar ratio of water-soluble aluminum salt, water-soluble magnesium salt and alkaline reagent is 1:3:12.

[0060] S104: After the microreactor reaction is completed, the mixed solution is transferred to a reactor containing 5.4 L of polyethylene glycol and 50 L of purified water, and stirred and mixed to obtain a slurry containing insoluble magnesium and aluminum hydroxides, namely, an insoluble slurry.

[0061] S105: With insoluble slurry as mobile phase, it enters into the reaction tube of microreactor at a feed flow rate of 10L / min. With carbon dioxide and air mixed gas as dispersed phase, it enters into the reactor body of microreactor at a feed flow rate of 12L / min, and then enters into the reaction tube after being dispersed through micropores at micron level on the side wall of the reactor body, wherein the carbon dioxide concentration in the mixed gas is 15%. The insoluble slurry and the mixed gas dispersed by micropores are fully mixed in the annular reaction tube, and the microwave generator assembly inside the microreactor is turned on. When the pH value of the material in the mixed reaction process reaches 10.3, the reaction is stopped to obtain a nanoscale reaction liquid.

[0062] S106: The filter cake obtained by filtering the reaction solution is washed with purified water and dried at 75° C. for 21 hours to obtain nano-scale aluminum carbonate.

[0063] Example 2

[0064] The present application embodiment provides a method for preparing nano-scale hydrotalcite based on a microreactor, the method comprising:

[0065] S201: Add 12.343 kg of potassium hydroxide to 100 kg of purified water, stir to dissolve, filter to a measuring kettle, and add the volume of the filtrate obtained by filtration to 110 L to obtain an alkali solution with a concentration of 2 mol / L.

[0066] S202: Add 6.84 kg aluminum sulfate and 7.2 kg magnesium sulfate to 90 kg purified water, stir to dissolve, filter to a measuring kettle, and add the volume of the filtrate obtained by filtration to 110 L to obtain a salt solution with a concentration of 0.73 mol / L.

[0067] S203: With saline as mobile phase, it enters into the reaction tube of the microreactor at a feed flow rate of 3L / min. With alkali solution as dispersed phase, it enters into the reactor body of the microreactor at a feed flow rate of 3L / min, and then enters into the reaction tube after being dispersed through micropores of micrometer level on the side wall of the reactor body. The saline solution and the small-particle alkali solution dispersed by the micropores are fully mixed in the annular reaction tube, and the microwave generator assembly inside the microreactor is turned on to react to obtain a mixed solution. Among them, the molar ratio of water-soluble aluminum salt, water-soluble magnesium salt and alkaline agent is 1:3:11.

[0068] S204: After the microreactor reaction is completed, the mixed solution is transferred to a reactor containing 5.4 L of polyvinyl alcohol and 50 L of purified water, and stirred and mixed to obtain a slurry containing insoluble magnesium and aluminum hydroxides, namely, an insoluble slurry.

[0069] S205: With insoluble slurry as mobile phase, it enters into the reaction tube of microreactor at a feed flow rate of 10L / min. With carbon dioxide and air mixed gas as dispersed phase, it enters into the reactor body of microreactor at a feed flow rate of 11L / min, and then enters into the reaction tube after being dispersed through micropores at micron level on the side wall of the reactor body, wherein the carbon dioxide concentration in the mixed gas is 10%. The insoluble slurry and the mixed gas dispersed by micropores are fully mixed in the annular reaction tube, and the microwave generator assembly inside the microreactor is turned on. When the pH value of the material reaches 11 during the mixed reaction, the reaction is stopped to obtain a nanoscale reaction liquid.

[0070] S206: The filter cake obtained by filtering the reaction solution is washed with purified water and dried at 70° C. for 22 hours to obtain nano-scale aluminum carbonate.

[0071] Example 3

[0072] The present application embodiment provides a method for preparing nano-scale hydrotalcite based on a microreactor, the method comprising:

[0073] S301: Add 11.2 kg of sodium hydroxide to 112 kg of purified water, stir to dissolve, and filter to a measuring kettle. The volume of the filtrate obtained by filtration is supplemented to 120 L to obtain an alkali solution with a concentration of 2.33 mol / L.

[0074] S302: Add 4.26 kg of aluminum nitrate and 5.71 kg of magnesium chloride to 100 kg of purified water, stir to dissolve, filter to a measuring kettle, and add the volume of the filtrate obtained by filtration to 120 L to obtain a salt solution with a concentration of 0.67 mol / L.

[0075] S303: With saline as mobile phase, it enters the reaction tube of the microreactor at a feed flow rate of 3L / min. With alkali solution as dispersed phase, it enters the reactor body of the microreactor at a feed flow rate of 3L / min, and then enters the reaction tube after being dispersed through micropores of micrometer level on the side wall of the reactor body. The saline solution and the small-particle alkali solution dispersed by the micropores are fully mixed in the annular reaction tube, and the microwave generator assembly inside the microreactor is turned on to react to obtain a mixed solution. Among them, the molar ratio of water-soluble aluminum salt, water-soluble magnesium salt and alkaline agent is 1:3:14.

[0076] S304: After the microreactor reaction is completed, the mixed solution is transferred to a reactor containing 5.4 L of cellulose acetate and 50 L of purified water, and stirred and mixed to obtain a slurry containing insoluble magnesium and aluminum hydroxides, namely, an insoluble slurry.

[0077] S305: With insoluble slurry as mobile phase, it enters into the reaction tube of microreactor at a feed flow rate of 10L / min. With carbon dioxide and air mixed gas as dispersed phase, it enters into the reactor body of microreactor at a feed flow rate of 15L / min, and then enters into the reaction tube after being dispersed through micropores at micron level on the side wall of the reactor body, wherein the carbon dioxide concentration in the mixed gas is 30%. The insoluble slurry and the mixed gas dispersed by micropores are fully mixed in the annular reaction tube, and the microwave generator assembly inside the microreactor is turned on. When the pH value of the material reaches 12 during the mixed reaction, the reaction is stopped to obtain a nanoscale reaction liquid.

[0078] S306: The filter cake obtained by filtering the reaction solution is washed with purified water and dried at 80° C. for 20 hours to obtain nano-scale aluminum carbonate.

[0079] Comparative Example 1: Preparation of saline solution using only water-soluble magnesium salt

[0080] D101: Add 4.8 kg of sodium hydroxide to 48 kg of purified water, stir to dissolve, and filter into a measuring kettle. Add the volume of the filtrate obtained by filtration to 60 L to obtain an alkali solution with a concentration of 2.0 mol / L.

[0081] D102: Add 5.71 kg of magnesium chloride to 50 kg of purified water, stir to dissolve, filter to a measuring kettle, and add the volume of the filtrate to 60 L to obtain a salt solution with a concentration of 1.0 mol / L.

[0082] D103: With saline as the mobile phase, it enters the reaction tube of the microreactor at a feed flow rate of 3L / min. With alkali as the dispersed phase, it enters the reactor body of the microreactor at a feed flow rate of 3L / min, and then enters the reaction tube after being dispersed through the micropores at the micron level on the side wall of the reactor body. The saline and the small-particle alkali dispersed by the micropores are fully mixed in the annular reaction tube, and the microwave generator assembly inside the microreactor is turned on to react to obtain a mixed solution.

[0083] D104: After the microreactor reaction is completed, the mixed solution is transferred to a reactor containing 2.67 kg aluminum chloride, 5.4 L polyethylene glycol and 150 L purified water, and stirred and mixed to obtain a slurry containing insoluble magnesium and aluminum hydroxide, namely, an insoluble slurry.

[0084] D105: With insoluble slurry as mobile phase, it enters into the reaction tube of microreactor at a feed rate of 10L / min. With carbon dioxide and air mixed gas as dispersed phase, it enters into the reactor body of microreactor at a feed rate of 12L / min, and then enters into the reaction tube after being dispersed through micropores at micron level on the side wall of the reactor body, wherein the carbon dioxide concentration in the mixed gas is 15%. The insoluble slurry and the mixed gas dispersed by micropores are fully mixed in the annular reaction tube, and the microwave generator assembly inside the microreactor is turned on. When the pH value of the material in the mixed reaction reaches 10.7, the reaction is stopped to obtain a nanoscale reaction liquid.

[0085] D106: The filter cake obtained by filtering the reaction solution was washed with purified water and dried at 75° C. for 21 h to obtain nano-scale aluminum carbonate.

[0086] Comparative Example 2: Only water-soluble aluminum salt is used to prepare the salt solution, and the magnesium salt is nano-magnesium hydroxide

[0087] D201: Add 4.8 kg of sodium hydroxide to 48 kg of purified water, stir to dissolve, filter into a measuring kettle, and add the volume of the filtrate to 60 L to obtain an alkali solution with a concentration of 2.0 mol / L.

[0088] D202: Add 2.67 kg aluminum chloride to 15 kg purified water, stir to dissolve, filter to a measuring kettle, and add the volume of the filtrate to 20 L to obtain a salt solution with a concentration of 1.0 mol / L.

[0089] D203: Magnesium hydroxide with a D90 of 254 nm and a mass of 3.5 kg was added into a reactor together with alkali solution, saline solution, 5.4 L of polyethylene glycol and 170 L of purified water, and stirred to obtain an insoluble slurry.

[0090] D204: With insoluble slurry as mobile phase, it enters into the reaction tube of microreactor at a feed rate of 10L / min. With carbon dioxide and air mixed gas as dispersed phase, it enters into the reactor body of microreactor at a feed rate of 12L / min, and then enters into the reaction tube after being dispersed through micropores at micron level on the side wall of the reactor body, wherein the carbon dioxide concentration in the mixed gas is 15%. The insoluble slurry and the mixed gas dispersed by micropores are fully mixed in the annular reaction tube, and the microwave generator assembly inside the microreactor is turned on. When the pH value of the material reaches 10.1 during the mixed reaction, the reaction is stopped to obtain a nanoscale reaction liquid.

[0091] D205: The filter cake obtained by filtering the reaction solution was washed with purified water and dried at 75° C. for 21 h to obtain nano-scale aluminum carbonate.

[0092] Comparative Example 3: Conventional preparation method

[0093] D301: Add 7.2 kg of sodium hydroxide and 3.18 kg of sodium carbonate to 100 kg of purified water, stir to dissolve, filter into a measuring kettle, and add the volume of the filtrate obtained by filtration to 110 L to obtain alkali solution.

[0094] D302: Add 2.67 kg aluminum chloride and 5.71 kg magnesium chloride to 85 kg purified water, stir to dissolve, filter to a measuring kettle, and add the volume of the filtrate to 110 L to obtain a salt solution.

[0095] D303: Slowly add the alkali solution and the salt solution to the reactor containing 5.4L polyethylene glycol and 50L purified water at the same time, control the dropping time to 1-1.5h, raise the temperature to 70-80℃, and keep the temperature for 3h. After the reaction is completed, stop heating and cool to room temperature in a water bath to obtain a reaction solution.

[0096] D304: The filter cake obtained by filtering the reaction solution was washed with purified water and dried at 75°C for 21 hours to obtain aluminum carbonate.

[0097] The particle size distribution of the hydrotalcite prepared in Example 1 and Comparative Examples 1-3 was measured by a particle size distribution measuring instrument to obtain the attached Figure 3-6 . Figure 3-6 It can be seen that the particle sizes of the hydrotalcite prepared in Example 1 and Comparative Examples 1-3 are: D90=191.2nm, D90=204.1nm, D90=390.6nm, and D90=262μm, respectively. It can be seen that, relative to the conventional preparation method of Comparative Example 3, the particle size of the hydrotalcite prepared in Example 1, Comparative Examples 1 and 2 using a microreactor reaches the nanometer level. That is, after using the microreactor in the embodiment of the present application, the particle size of the hydrotalcite prepared all reaches the nanometer level.

[0098] In addition, for different raw materials, although the particle size of hydrotalcite prepared in Comparative Examples 1 and 2 reaches nanometer level, the particle size of hydrotalcite prepared in Example 1 is lower. This shows that the selection of raw materials has an important influence on the particle size of hydrotalcite.

[0099] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing nano-scale hydrotalcite based on a microreactor, characterized in that: include: Adding alkaline reagent into purified water, stirring to dissolve, filtering to obtain alkaline solution; Adding water-soluble aluminum salt and water-soluble magnesium salt into purified water, stirring to dissolve, filtering, and obtaining a salt solution; The salt solution is used as a mobile phase to enter the reaction tube of the microreactor, and the alkali solution is used as a dispersed phase to enter the interior of the reactor body of the microreactor, and then enters the reaction tube through the micropores on the side wall of the reactor body, and the salt solution and the alkali solution are mixed and reacted in a countercurrent mass transfer in the reaction tube to obtain a mixed solution; The mixed liquid is stirred and mixed with a water-soluble dispersant to obtain an insoluble slurry; The insoluble slurry is used as a mobile phase to enter the reaction tube of the microreactor, and the mixed gas of carbon dioxide and air is used as a dispersed phase to enter the reactor body of the microreactor, and then enters the reaction tube through the micropores on the side wall of the reactor body. The insoluble slurry and the mixed gas are mixed and reacted in the reaction tube in a countercurrent mass flow. When the pH value of the material in the mixed reaction process reaches 10-12, the reaction is stopped to obtain a reaction solution; The reaction solution is filtered, washed and dried to obtain nano-scale hydrotalcite; The microreactor comprises a reactor body (1), a reaction tube (2) and a microwave generator assembly (3) which are arranged in a sealed manner from the outside to the inside, wherein a micropore (4) is provided on the tube wall of the reaction tube (2); after the dispersed phase enters the reactor body (1) and passes through the micropore (4), it reacts with the mobile phase in a countercurrent mass transfer manner in the cavity between the reaction tube (2) and the microwave generator assembly (3); The angle between the opening direction of the micropore (4) and the flow direction of the mobile phase is 0-90°, and the diameter of the micropore (4) is 1-2000 μm.

2. The method for preparing nano-scale hydrotalcite based on a microreactor according to claim 1, characterized in that: The molar ratio of the water-soluble aluminum salt, the water-soluble magnesium salt and the alkaline agent is 1:3:(11-14).

3. The method for preparing nano-scale hydrotalcite based on a microreactor according to claim 1, characterized in that: The alkaline agent includes sodium hydroxide or potassium hydroxide; the water-soluble aluminum salt includes aluminum chloride, aluminum sulfate or aluminum nitrate; and the water-soluble magnesium salt includes magnesium sulfate or magnesium chloride.

4. The method for preparing nano-scale hydrotalcite based on a microreactor according to claim 1, characterized in that: The water-soluble dispersant includes polyethylene glycol, polyvinyl alcohol, cellulose acetate or polyvinyl pyrrolidone.

5. The method for preparing nano-scale hydrotalcite based on a microreactor according to claim 1, characterized in that: The concentration of carbon dioxide in the mixed gas is 10-30%.

6. The method for preparing nano-scale hydrotalcite based on a microreactor according to claim 1, characterized in that: The drying temperature is 70-80°C and the drying time is 20-22h.

7. The method for preparing nano-scale hydrotalcite based on a microreactor according to claim 1, characterized in that: The feed flow rate ratio of the salt solution to the alkali solution is 1:1, and the feed molar concentration ratio is 1:(2.75-3.5); the feed flow rate ratio of the insoluble slurry to the mixed gas is 1:(1.1-1.5).

8. The method for preparing nano-scale hydrotalcite based on a microreactor according to claim 1, characterized in that: The microwave generator assembly (3) comprises a microwave-transmissive generator sleeve (301), a microwave generator (302) clamped on the inner wall of the generator sleeve (301), and a microwave controller (303) electrically connected to the microwave generator (302); the generator sleeve (301) is fixed to the inner wall of the reaction tube (2) via a supporting foot (5), and the microwave controller (303) is located outside the reactor body (1).

Citation Information

Patent Citations

  • Method for preparing nano magnalium hydrotalcite and equipment thereof

    CN101381094A

  • Nano magnesium-aluminum hydrotalcite and preparation method thereof

    CN106379924A

  • Nano hydrotalcite crystal suspension and preparation method thereof

    CN112274532A

  • Crystallization method of micron-sized hydrotalcite with narrow particle size distribution

    CN116102046A

  • Laminar bimetal hydroxide and preparation method thereof

    CN102976278A