High-salt-resistant and high-temperature-resistant instant associative thickener for fracturing and preparation method thereof
By introducing salt-resistant sulfonic acid groups, high-temperature resistant two-dimensional planar structures and strong hydrophilic groups into the associative thickener, the lack of performance of associative thickener in high salt and high temperature is solved, and the rapid development of the associative thickener is achieved. Sticky and efficient and stable performance.
Patent Information
- Application Number
- CN202410981067.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-22
AI Technical Summary
The existing associative thickeners for fracturing are insufficient in high salt and high temperature conditions and have low dissolution rate, making it difficult to ensure the overall performance of deep oil and gas reservoir transformation.
By introducing polymerizable modified graphene oxide functional monomers that are resistant to salt sulfonic acid groups, high temperature resistant two-dimensional planar structures and strong hydrophilic groups, the high salt resistant, high temperature and instant melting properties of the associative thickener are improved.
It significantly improves the high salt resistance, high temperature and instant melting properties of the associative thickener, ensuring high-efficiency performance under high mineralization and high temperature conditions, including rapid viscosity, stable viscosity and high thixotropic energy.
Smart Images

Figure CN118496448B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas production enhancement, and is a high-salt and high-temperature resistant instant associative thickener for fracturing and a preparation method thereof. Background Art
[0002] Fracturing and production increase is an important technical means to achieve the scale and efficiency development of unconventional resources such as tight oil and gas, and it has important practical significance for ensuring the increase of reserves and production of oil and gas resources and the stable and continuous supply of energy in my country. Fracturing fluid is a chemical working fluid that must be used in the process of fracturing and production increase. The quality of its performance will significantly affect the final transformation effect and oil and gas recovery rate to a large extent. As an important main agent of fracturing fluid, the temperature and salt resistance of thickeners are particularly critical to ensure the drag reduction and sand carrying properties of fracturing fluid systems. Due to its good drag reduction, strong thickening ability, low residue content, and insensitivity to bacteria, synthetic polymers have become one of the mainstream directions for the research and application of fracturing fluid thickeners. With the continuous advancement of the reservoir transformation process and the continuous expansion of its scale, fracturing and production increase are advancing into deep oil and gas with greater burial depth, higher temperature and formation mineralization, and the need to repeatedly prepare fracturing fluid using flowback fluid on site is very urgent, which poses a great challenge to the salt resistance of fracturing fluid thickeners. At the same time, the continuous mixing process currently widely used on site to shorten the fracturing construction cycle and reduce operating costs also places higher requirements on the solubility of fracturing fluid thickeners.
[0003] At present, conventional polyacrylamide polymers are the most mature synthetic polymers, but the salt resistance of this type of polymer in practical applications is very limited. Under high mineralization conditions (especially in the presence of high-temperature high-valent ions), the viscosity loss is obvious or even flocculation precipitation occurs, and the overall viscoelasticity and sand carrying capacity are significantly reduced. Associative polymers can significantly enhance the structural strength, viscosity enhancement and viscoelasticity through the interaction between associative groups in aqueous solution, and the presence of salt metal ions can further promote this associative effect at a certain mineralization. Therefore, they have been widely studied and applied to fracturing and production enhancement operations under saline conditions on a certain scale. However, the improvement of the salt resistance of the thickener by associative action alone is also very limited, and the greater the salt resistance requirement, the higher the content of associative groups required. At the same time, the associative action also leads to the problems of low dissolution rate, easy formation of fish eyes, slow viscosity, etc. in the fracturing fluid formed by associative polymers as thickeners, and the higher the content of associative groups, the more unfavorable it is for solubility. It is often necessary to add additional quick-dissolving aids to improve solubility, which will inevitably lead to complex preparation process, incompatibility with other fracturing additives, and possible chromatographic separation in application. In addition, under high temperature conditions, associative thickeners will show a much more obvious performance decline trend than under medium and low temperature conditions, and their temperature resistance is limited. Therefore, the preparation of fast-dissolving fracturing thickeners with strong salt tolerance and high temperature resistance is of great significance to ensure the efficient development of deep oil and gas and the reuse of return fluids, and has become an important direction for continuous research in the field of fracturing production increase technology.
[0004] A Chinese patent document with authorization announcement number CN115947891B discloses a heat-resistant and salt-resistant instant polyacrylamide and a preparation method and application thereof. The polyacrylamide is modified by introducing a rigid heat-resistant and salt-resistant monomer containing a benzene ring and a fluorine-containing cationic hydrophobic monomer on the basis of acrylamide monomer and sodium acrylate monomer, and a narrow distribution of medium and low molecular weight polyacrylamide is prepared by synthetic instant dissolving technology and ATRP polymerization method. Under clear water conditions, 0.03% powder can become sticky within 48 seconds, and the viscosity of 0.1%-0.3% powder at a mineralization of 100,000 mg / L (calcium and magnesium ions 20,000 mg / L) and room temperature is as high as 13.57-27.75 mPa·s.
[0005] A Chinese patent document with publication number CN116285936A discloses a high temperature resistant and salt resistant instant fracturing fluid thickener and a preparation method thereof. The polyacrylamide is modified by introducing carboxylic acid group-containing monomers, salt resistant monomers containing benzenesulfonic acid groups or benzoic acid groups, and fluorine-containing cationic hydrophobic monomers into the molecular structure of polyacrylamide. The carboxylic acid group-containing or sulfonic acid group-containing monomers can improve the solubility and salt resistance of the thickener, the monomers containing benzene ring groups can improve the heat resistance and shear resistance of the thickener, and the fluorine-containing cationic hydrophobic monomers can improve the viscosity and heat resistance and shear resistance of the thickener. Under clear water conditions, 0.03% powder can become sticky within 47 seconds, and the viscosity of 0.1%-0.2% powder at a mineralization of 120,000 mg / L (calcium and magnesium ions 10,000 mg / L) and room temperature is as high as 15.49-27.86 mPa·s.
[0006] A Chinese patent document with authorization announcement number CN114716606B discloses a heat-resistant and salt-resistant fast-dissolving polymer for oil displacement and a preparation method thereof. Acrylamide, sulfonic acid group-containing monomers, quaternary ammonium group-containing monomers, weakly branched monomers and polymerization aids (chain extenders, chain transfer agents, small molecule aids, dispersing aids, reducing agents, etc.) are introduced into the polymer. The mineralization is 32868 mg / L (calcium and magnesium ions are unknown). At 70°C, the viscosity of 0.25% polymer is as high as 35.9 mPa·s, and the mineralization is 8421 mg / L (calcium and magnesium ions are 200 mg / L). It can be completely dissolved within 20 to 30 minutes at room temperature.
[0007] A Chinese patent document with authorization announcement number CN111635749A discloses a slippery water system that takes into account both drag reduction and sand carrying, and a preparation method thereof. The system improves salt resistance by introducing salt-resistant monomer units 2-acrylamide-2-methacrylic acid and / or 2-acrylamide-2-methacrylate sodium into the associative polymer structural unit, and adds a co-solvent to improve solubility. At a mineralization of 100,000 mg / L (calcium and magnesium ions 5,600 mg / L), 0.15% drag reducer is uniformly dissolved in 3 minutes and has a viscosity of 5.6 mPa·s.
[0008] A Chinese patent document with authorization announcement number CN106190088B discloses a heat-resistant and salt-resistant quick-dissolving thickener for seawater-based fracturing fluid and a preparation method thereof. The heat-resistant and salt-resistant quick-dissolving thickener is prepared by copolymerization of acrylic acid, acrylamide, an isolation monomer, a functional anion monomer (2-acrylamide-2-methylpropanesulfonic acid or sodium methacrylate), a functional cationic monomer (dimethyldiallyl ammonium chloride, hexadecyldimethylallyl ammonium chloride or octadecyl methacrylate), and an associative intermediate (introducing double bonds into p-aminobenzenesulfonic acid, p-toluenesulfonic acid, and p-vinylbenzenesulfonic acid). The dissolution time is ≤10min at a mineralization of 45000mg / L (calcium and magnesium ions 2720mg / L) and room temperature, and the viscosity is ≥80mPa·s at a dosage of 0.5%. The viscosity is 120℃ and 170s -1 The low temperature and shear resistance viscosity is about 45mPa·s.
[0009] A Chinese patent document with authorization announcement number CN105085801B discloses a fast-soluble polyacrylamide and a preparation method thereof. The fast-soluble polyacrylamide is prepared by copolymerizing acrylamide, carboxyl group-containing monomers (acrylic acid, methacrylic acid, methylene succinic acid and 3-acrylamide-3-methylbutyric acid), sulfonic acid group-containing monomers (sodium methyl propylene sulfonate, sodium allyl sulfonate, sodium vinyl sulfonate, 2-methyl-2-acrylic acid-2-sulfoethyl ester and sodium 2-acrylamide-2-methylpropane sulfonate) with modified cellulose, and adding a cosolvent, a chain extender, a chain transfer agent and a metal complexing agent. The dissolution time is 10-20 minutes at 20°C-40°C.
[0010] Wang Chao and others from the China Petroleum Exploration and Development Research Institute used acrylamide, 2-acrylamide-2-methylpropane sulfonic acid and functional monomer SP to copolymerize, and added chain transfer agents, urea and other additives to prepare a slow-crosslinking ultra-high temperature synthetic polymer fracturing fluid thickener. The fluid began to become sticky 30 seconds after adding 0.5% of it in clean water at room temperature, and the viscosity reached 94.7% of the stable viscosity (58 mPa·s) in 8 minutes (Wang Chao, Research on Slow-crosslinking Ultra-high Temperature Synthetic Polymer Fracturing Fluid Thickener, Drilling Fluids and Completion Fluids, 2022, 39 (03)).
[0011] Liu Tongyi et al. from Southwest Petroleum University prepared a fracturing fluid thickener by copolymerizing acrylamide, N-hydroxymethyl acrylamide (NMA) and hydrophobic cationic monomers. At 1% KCl and 100°C, 0.35% of the polymer was almost completely dissolved within 40 minutes, and the viscosity was stable (greater than 53 mPa·s) at 60 minutes (Liu Tongyi et al., Synthesis and Evaluation of an Aluminum Cross-linked Fracturing Fluid Thickener, Petrochemical Engineering, 2018, 47 (2)).
[0012] The above existing patents and public research mainly introduce acrylamide alkyl sulfonic acid and its sulfonate, sulfonic acid or sulfonate with rigid structure (such as sodium styrene sulfonate) into the associative thickener macromolecule to improve its salt and temperature resistance. At the same time, by adding non-reactive fast-dissolving aids in the synthesis process and technology of the thickener, it does not involve introducing monomers containing salt-resistant sulfonic acid groups, high-temperature resistant two-dimensional planar structures, and strong hydrophilic groups into the associative thickener to simultaneously solve the problems of high salt resistance, high temperature resistance, and fast dissolution. The salt resistance, temperature resistance and dissolution resistance that can be achieved by conventional methods still have a lot of room for improvement. Summary of the invention
[0013] The present invention provides a high-salt and high-temperature resistant instant associative thickener for fracturing and a preparation method thereof, which overcomes the deficiencies of the above-mentioned prior art and can effectively solve the problems of insufficient high-salt and high-temperature resistance, low dissolution rate, and difficulty in ensuring the overall performance of fracturing fluid in the transformation of deep layers with high mineralization and unconventional oil and gas reservoirs of the existing associative thickeners for fracturing.
[0014] One of the technical solutions of the present invention is achieved through the following measures: a high-salt and high-temperature resistant fast-dissolving associative thickener for fracturing, the raw materials of which include acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups, wherein the mass ratio of acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups is: 1: 0.15 to 0.3: 0.005 to 0.05: 0.00005 to 0.0005.
[0015] The following is a further optimization and / or improvement of one of the above-mentioned technical solutions:
[0016] The above-mentioned associative monomer containing unsaturated double bonds and amphiphilic groups is one or more of long-chain alkyl unsaturated quaternary ammonium salts and N-alkyl substituted acrylamide associative monomers. The structural formula of the associative monomer containing unsaturated double bonds and amphiphilic groups is:
[0017] .
[0018] The above R1 structural formula is:
[0019] , One of the foregoing, wherein m is an integer from 11 to 19, n is an integer from 0 to 4, and z is an integer from 1 to 2.
[0020] The above R2 structural formula is:
[0021] , wherein n is an integer from 11 to 19.
[0022] The structural formula of the above-mentioned polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is:
[0023] .
[0024] The above R3 structural formula is:
[0025] , where n is an integer from 0 to 1.
[0026] The above R4 structural formula is:
[0027] , where n is an integer from 0 to 1.
[0028] The above-mentioned polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is obtained according to the following method:
[0029] The first step is to ultrasonically disperse the required amount of graphene oxide with an ethanol aqueous solution having a mass concentration of 90% to 95%, add the required amount of a silane coupling agent containing an unsaturated double bond at 55° C. to 65° C. and continuously stir, and reflux for 6 h to 8 h to obtain a first reaction mixture;
[0030] The second step is to cool the reaction mixture to room temperature overnight, vacuum filter and wash twice with acetone, and dry at 50° C. to 70° C. for 17 to 18 hours to obtain a modified graphene oxide intermediate containing unsaturated double bonds;
[0031] The third step is to ultrasonically treat the required amount of the modified graphene oxide intermediate with unsaturated double bonds in deionized water for 1.5 to 2.5 hours to obtain a uniform intermediate dispersion;
[0032] Step 4: dissolving the required amount of 6-amino-4-hydroxy-2-naphthalenesulfonate in deionized water pre-added with 0.2 mL to 0.5 mL of aqueous ammonia, and then adding it to the intermediate dispersion under continuous stirring, and refluxing at 70° C. to 80° C. for 8 h to 9 h to obtain a second reaction mixture;
[0033] The fifth step is to cool the second reaction mixture to room temperature and stand it for 8 hours, centrifuge it at 1200r / min in a high-speed centrifuge for 15 to 20 minutes, separate the upper liquid, and wash the upper liquid three times with 60% to 70% ethanol aqueous solution and pure water to obtain a polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group.
[0034] In the first step, the mass ratio of graphene oxide to the silane coupling agent containing an unsaturated double bond is 1:1.5 to 2, and the silane coupling agent containing an unsaturated double bond is one or more of vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, and allyltriethoxysilane;
[0035] In the fourth step, the molar concentration of ammonia water is 1 mol / L, and the mass ratio of the modified graphene oxide intermediate containing unsaturated double bonds to 6-amino-4-hydroxy-2-naphthalenesulfonate is 1:2 to 3.
[0036] The high-salt and high-temperature resistant instant associative thickener for fracturing is obtained according to the following method:
[0037] S1, mixing and dissolving required amounts of acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups in water to obtain a mixed solution with a mass concentration of 18% to 28%;
[0038] S2, adjusting the pH value of the mixed solution to 7 to 8 with a pH adjuster, refrigerating the mixed solution for 30 minutes to lower the temperature to -5°C, and then adding a required amount of a low-temperature composite initiator to initiate a polymerization reaction to obtain a colloidal product;
[0039] S3, chopping, sieving and drying the colloidal product to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing.
[0040] In the above step S2, the pH adjuster is one or more of sodium bicarbonate, sodium hydroxide, potassium hydroxide, citric acid, and glacial acetic acid, the low-temperature composite initiator is a mixture of sodium persulfate, sodium bisulfite and an inorganic compound oxidant in a volume ratio of 1:1:0.1, the volume ratio of the low-temperature composite initiator to the mixed solution is 1:250, and the polymerization reaction temperature is -5°C to 20°C, wherein the inorganic compound oxidant is one or more of ammonium cerium nitrate and ammonium cerium sulfate.
[0041] The second technical solution of the present invention is achieved by the following measures: a method for preparing a high-salt and high-temperature resistant instant associative thickener for fracturing, which is carried out according to the following method:
[0042] S1, mixing and dissolving required amounts of acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups in water to obtain a mixed solution with a mass concentration of 18% to 28%;
[0043] S2, adjusting the pH value of the mixed solution to 7 to 8 with a pH regulator, refrigerating the mixed solution for 30 minutes to reduce the temperature of the mixed solution to -5°C, and then adding a required amount of a low-temperature composite initiator to initiate a polymerization reaction to obtain a colloidal product, wherein the pH regulator is one or more of sodium bicarbonate, sodium hydroxide, potassium hydroxide, citric acid, and glacial acetic acid, the low-temperature composite initiator is a mixture of sodium persulfate, sodium bisulfite and an inorganic compound oxidant in a volume ratio of 1:1:0.1, the volume ratio of the low-temperature composite initiator to the mixed solution is 1:250, the polymerization reaction temperature is -5°C to 20°C, and the inorganic compound oxidant is one or more of ammonium cerium nitrate and ammonium cerium sulfate;
[0044] S3, chopping, sieving and drying the colloidal product to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing.
[0045] The present invention introduces a monomer containing a salt-resistant sulfonic acid group, a high-temperature resistant two-dimensional planar structure, and a strong hydrophilic group into the macromolecular skeleton of the associative thickener, thereby simultaneously improving the high salt resistance, high temperature resistance and quick dissolution performance of the associative thickener. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Attached Figure 1 ] are infrared spectra of graphene oxide (GO) before modification and graphene oxide (NMGO) after modification in Example 14 of the present invention.
[0047] Attached Figure 2 This is a comparison chart of the temperature and shear resistance of the high-salt and high-temperature resistant instant associative thickener for fracturing prepared in Example 23 of the present invention at a concentration of 1.5% and that of Comparative Example 2.
[0048] Attached Figure 3 This is a comparison chart of the temperature and shear resistance of the high-salt and high-temperature resistant instant associative thickener for fracturing prepared in Example 25 of the present invention at a concentration of 1.5% and that of Comparative Example 4.
[0049] Attached Figure 4 This is a comparison chart of the thixotropic energy of the high-salt and high-temperature resistant instant associative thickener for fracturing prepared in Example 23 and Example 25 of the present invention at a concentration of 1.5% and that of Comparative Examples 2 and 4. DETAILED DESCRIPTION
[0050] The present invention is not limited by the following embodiments, and the specific implementation method can be determined according to the technical scheme of the present invention and the actual situation. Unless otherwise specified, the various chemical reagents and chemicals mentioned in the present invention are all chemical reagents and chemicals known and used in the prior art; unless otherwise specified, the percentages in the present invention are all mass percentages; unless otherwise specified, the solutions in the present invention are all aqueous solutions with water as the solvent, for example, hydrochloric acid solution is a hydrochloric acid aqueous solution; the normal temperature and room temperature in the present invention generally refer to a temperature of 15°C to 25°C, and are generally defined as 25°C.
[0051] The present invention will be further described below in conjunction with embodiments:
[0052] Embodiment 1: The high-salt and high-temperature resistant fast-dissolving associative thickener for fracturing, the raw materials include acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups, wherein the mass ratio of acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups is: 1: 0.15 to 0.3: 0.005 to 0.05: 0.00005 to 0.0005.
[0053] The present invention introduces a salt-resistant sulfonic acid group, a high-temperature resistant two-dimensional planar structure (a polymerizable modified graphene oxide functional monomer containing a sulfonic acid group and a hydroxyl group), and a strong hydrophilic group monomer into the macromolecular skeleton of the associative thickener, thereby simultaneously improving the high salt resistance, high temperature resistance and quick dissolution performance of the associative thickener. Among them, the molecular weight range of the high-salt and high-temperature resistant quick-dissolving associative thickener for fracturing of the present invention is 5 million Daltons to 15 million Daltons, the mineralization is 150,000 mg / L (calcium and magnesium ion content is 15,000 mg / L), 0.2% to 1.5% thickener becomes sticky within 25 seconds at room temperature, the 2-minute viscosity release rate is greater than 90% and there are no insoluble particles, and the viscosity is 12 Pa·s to 132 mPa·s; under the same mineralization and divalent ion content, at 180°C, 1.5% thickener becomes sticky within 170 seconds -1 After 2 hours of shearing, the viscosity reaches 61mPa·s and the thixotropic energy reaches 1000Pa / s.
[0054] Embodiment 2: As an optimization of the above embodiment, the associative monomer containing an unsaturated double bond and an amphiphilic group is one or more of a long-chain alkyl unsaturated quaternary ammonium salt and an N-alkyl substituted acrylamide associative monomer, and the structural formula of the associative monomer containing an unsaturated double bond and an amphiphilic group is:
[0055] .
[0056] Embodiment 3: As an optimization of the above embodiment, the structural formula of R1 is:
[0057] , One of the foregoing, wherein m is an integer from 11 to 19, n is an integer from 0 to 4, and z is an integer from 1 to 2.
[0058] Embodiment 4: As an optimization of the above embodiment, the structural formula of R2 is:
[0059] , wherein n is an integer from 11 to 19.
[0060] Example 5: As an optimization of the above example, the structural formula of the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is:
[0061] .
[0062] Embodiment 6: As an optimization of the above embodiment, the structural formula of R3 is:
[0063] , where n is an integer from 0 to 1.
[0064] Embodiment 7: As an optimization of the above embodiment, the structural formula of R4 is:
[0065] , where n is an integer from 0 to 1.
[0066] Example 8: As an optimization of the above example, a polymerizable modified graphene oxide functional monomer containing a sulfonic acid group and a hydroxyl group is obtained according to the following method:
[0067] The first step is to ultrasonically disperse the required amount of graphene oxide with an ethanol aqueous solution having a mass concentration of 90% to 95%, add the required amount of a silane coupling agent containing an unsaturated double bond at 55° C. to 65° C. and continuously stir, and reflux for 6 h to 8 h to obtain a first reaction mixture;
[0068] The second step is to cool the first reaction mixture to room temperature overnight, vacuum filter and wash twice with acetone, and dry at 50° C. to 70° C. for 17 to 18 hours to obtain a modified graphene oxide intermediate containing unsaturated double bonds;
[0069] The third step is to ultrasonically treat the required amount of the modified graphene oxide intermediate with unsaturated double bonds in deionized water for 1.5 to 2.5 hours to obtain a uniform intermediate dispersion;
[0070] Step 4: dissolving the required amount of 6-amino-4-hydroxy-2-naphthalenesulfonate in deionized water pre-added with 0.2 mL to 0.5 mL of aqueous ammonia, and then adding it to the intermediate dispersion under continuous stirring, and refluxing at 70° C. to 80° C. for 8 h to 9 h to obtain a second reaction mixture;
[0071] The fifth step is to cool the second reaction mixture to room temperature and stand it for 8 hours, centrifuge it at 1200r / min in a high-speed centrifuge for 15 to 20 minutes, separate the upper liquid, and wash the upper liquid three times with 60% to 70% ethanol aqueous solution and pure water to obtain a polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group.
[0072] Example 9: As an optimization of the above example, in the first step, the mass ratio of graphene oxide to the silane coupling agent containing unsaturated double bonds is 1:1.5 to 2, and the silane coupling agent containing unsaturated double bonds is one or more of vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, and allyltriethoxysilane.
[0073] Example 10: As an optimization of the above example, in the fourth step, the molar concentration of ammonia water is 1 mol / L, and the mass ratio of the modified graphene oxide intermediate containing unsaturated double bonds to 6-amino-4-hydroxy-2-naphthalenesulfonate is 1:2 to 3.
[0074] Embodiment 11: As an optimization of the above embodiment, the following method is used to obtain:
[0075] S1, mixing and dissolving required amounts of acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups in water to obtain a mixed solution with a mass concentration of 18% to 28%;
[0076] S2, adjusting the pH value of the mixed solution to 7 to 8 with a pH adjuster, refrigerating the mixed solution for 30 minutes to lower the temperature to -5°C, and then adding a required amount of a low-temperature composite initiator to initiate a polymerization reaction to obtain a colloidal product;
[0077] S3, chopping, sieving and drying the colloidal product to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing.
[0078] Example 12: As an optimization of the above example, in step S2, the pH adjuster is one or more of sodium bicarbonate, sodium hydroxide, potassium hydroxide, citric acid, and glacial acetic acid, the low-temperature composite initiator is a mixture of sodium persulfate, sodium bisulfite and an inorganic compound oxidant in a volume ratio of 1:1:0.1, the volume ratio of the low-temperature composite initiator to the mixed solution is 1:250, and the polymerization reaction temperature is -5°C to 20°C, wherein the inorganic compound oxidant is one or more of ammonium ceric nitrate and ammonium ceric sulfate.
[0079] Example 13: The preparation method of the high-salt-resistant and high-temperature-resistant instant associative thickener for fracturing is carried out according to the following method:
[0080] S1, mixing and dissolving required amounts of acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups in water to obtain a mixed solution with a mass concentration of 18% to 28%;
[0081] S2, adjusting the pH value of the mixed solution to 7 to 8 with a pH regulator, refrigerating the mixed solution for 30 minutes to reduce the temperature of the mixed solution to -5°C, and then adding a required amount of a low-temperature composite initiator to initiate a polymerization reaction to obtain a colloidal product, wherein the pH regulator is one or more of sodium bicarbonate, sodium hydroxide, potassium hydroxide, citric acid, and glacial acetic acid, the low-temperature composite initiator is a mixture of sodium persulfate, sodium bisulfite and an inorganic compound oxidant in a volume ratio of 1:1:0.1, the volume ratio of the low-temperature composite initiator to the mixed solution is 1:250, the polymerization reaction temperature is -5°C to 20°C, and the inorganic compound oxidant is one or more of ammonium cerium nitrate and ammonium cerium sulfate;
[0082] S3, chopping, sieving and drying the colloidal product to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing.
[0083] Example 14: A polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is obtained according to the following method:
[0084] In the first step, 0.8 g of graphene oxide was dispersed in 200 mL of 95% ethanol aqueous solution under ultrasound, and stirred continuously at 60° C. and 450 r / min, and 1.6 g of vinyltrimethoxysilane containing unsaturated double bonds was slowly added and refluxed for 6 h to obtain a first reaction mixture;
[0085] In the second step, the first reaction mixture was cooled to room temperature and allowed to stand for 18 hours, vacuum filtered and washed twice with acetone, and dried at 65° C. for 18 hours to obtain a modified graphene oxide intermediate containing unsaturated double bonds (hereinafter referred to as MGO-1);
[0086] In the third step, 0.5 g of MGO-1 was ultrasonicated in 200 mL of deionized water for 2 h to form a uniform intermediate dispersion;
[0087] Step 4: dissolving 1.5 g of sodium 6-amino-4-hydroxy-2-naphthalenesulfonate in deionized water to which 0.3 mL of ammonia water (molar concentration of 1 mol / L) has been previously added, slowly adding the solution to the intermediate dispersion under continuous stirring, and reacting under reflux at 75° C. for 8.5 h to obtain a second reaction mixture;
[0088] In the fifth step, the second reaction mixture was cooled to room temperature and allowed to stand for 8 hours, and then centrifuged at 1200 r / min for 20 minutes using a high-speed centrifuge to separate the upper layer, and the upper layer was washed three times with a 70% ethanol aqueous solution and pure water to obtain polymerizable modified graphene oxide containing sulfonic acid groups and hydroxyl groups (hereinafter referred to as NMGO-1).
[0089] The graphene oxide before modification (ie, GO) and the graphene oxide after modification (ie, NMGO-1) in Example 14 of the present invention were characterized by Fourier transform infrared spectroscopy using a KBr pellet method. The results are as follows: Figure 1 shown. Figure 1 It can be seen that the absorption peaks of modified NMGO-1 corresponding to graphene oxide have mostly blue-shifted to a certain extent, at 1396 cm -1 The hydroxyl bending vibration peak corresponding to 2923 cm -1 and 2851cm -1 New characteristic absorption peaks at 1622cm- -1 The absorption peak attributable to the carbon-carbon double bond (C=C) in NMGO-1 red-shifts to 1593 cm -1 At 1383cm -1 The stretching vibration peak of the carbon-nitrogen bond (CN) appeared at 1183 cm -1 、1101cm -1 、1041cm -1 The stretching vibration peaks of the naphthalene ring and the sulfonic acid group appear at the positions respectively, confirming the successful preparation of the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group.
[0090] Example 15: The method of Example 14 was followed, except that the silane coupling agent containing unsaturated double bonds was replaced with allyltrimethoxysilane to prepare polymerizable modified graphene oxide NMGO-2 containing sulfonic acid groups and hydroxyl groups; the successful preparation of polymerizable modified graphene oxide containing sulfonic acid groups and hydroxyl groups was also confirmed by Fourier transform infrared spectroscopy characterization.
[0091] Example 16: The high-salt and high-temperature resistant instant associative thickener for fracturing is obtained according to the following method:
[0092] S1, acrylamide hydrophilic monomer (acrylamide), sodium acrylate hydrophilic monomer (sodium acrylate), associative monomer containing unsaturated double bonds and amphiphilic groups (hexadecyl dimethyl allyl ammonium chloride) and NMGO-1 obtained in Example 14 are mixed in a mass ratio of 1:0.15:0.005:0.00005, and a mixed solution with a total monomer mass concentration of 25% is prepared in a 1000 mL beaker with clean water;
[0093] S2, adding a pH regulator (sodium bicarbonate) to the mixed solution to adjust the pH value to 7, stirring evenly and cooling to -5°C, taking out the mixed solution and transferring it to an adiabatic polymerization device, adding 2 mL of a low-temperature composite initiator to initiate the polymerization reaction, and inserting an electronic thermometer to monitor the reaction temperature. When the temperature rises to the highest and then drops to a value that does not exceed 1°C, the reaction is terminated to obtain a colloidal product;
[0094] S3, taking out the obtained colloidal product and cutting it into small particles of about 5 mm, placing it on a 80-mesh sieve, drying it at 95°C and sieving it to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing (i.e., NYKWSR-1) with a mesh number ≥ 80 mesh.
[0095] The viscosity average molecular weight of NYKWSR-1 obtained in Example 16 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 14.78 million Daltons.
[0096] Example 17: The method of Example 16 was followed, except that the mass ratio of acrylamide, sodium acrylate, hexadecyl dimethyl allyl ammonium chloride and NMGO-1 was changed to 1:0.3:0.005:0.00005 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing (i.e., NYKWSR-2) with a mesh size ≥80.
[0097] The viscosity average molecular weight of NYKWSR-2 obtained in Example 17 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 14.5 million Daltons.
[0098] Example 18: The method of Example 16 was followed, except that the mass ratio of acrylamide, sodium acrylate, hexadecyl dimethyl allyl ammonium chloride and NMGO-1 was changed to 1:0.15:0.05:0.00005 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing (i.e., NYKWSR-3) with a mesh size ≥80.
[0099] The viscosity average molecular weight of NYKWSR-3 obtained in Example 18 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 13.25 million Daltons.
[0100] Example 19: The method of Example 16 was followed, except that the mass ratio of acrylamide, sodium acrylate, hexadecyl dimethyl allyl ammonium chloride and NMGO-1 was changed to 1:0.3:0.05:0.00005 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing with a mesh size of ≥80 (i.e., NYKWSR-4).
[0101] The viscosity average molecular weight of NYKWSR-4 obtained in Example 19 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 11.47 million Daltons.
[0102] Example 20: The method of Example 16 was followed, except that the mass ratio of acrylamide, sodium acrylate, hexadecyl dimethyl allyl ammonium chloride and NMGO-1 was changed to 1:0.15:0.005:0.0005 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing (i.e., NYKWSR-5) with a mesh size ≥80.
[0103] The viscosity average molecular weight of NYKWSR-5 obtained in Example 20 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 10.24 million Daltons.
[0104] Example 21: The method of Example 16 is followed, except that the mass ratio of acrylamide, sodium acrylate, hexadecyl dimethyl allyl ammonium chloride and NMGO-1 is changed to 1:0.3:0.005:0.0005 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing (i.e., NYKWSR-6) with a mesh size ≥80.
[0105] The viscosity average molecular weight of NYKWSR-6 obtained in Example 21 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 8.96 million Daltons.
[0106] Example 22: The method of Example 16 is followed, except that the mass ratio of acrylamide, sodium acrylate, hexadecyl dimethyl allyl ammonium chloride and NMGO-1 is changed to 1:0.15:0.05:0.0005 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing (i.e., NYKWSR-7) with a mesh size ≥80.
[0107] The viscosity average molecular weight of NYKWSR-7 obtained in Example 22 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 7.54 million Daltons.
[0108] Example 23: The method of Example 16 was followed, except that the mass ratio of acrylamide, sodium acrylate, hexadecyl dimethyl allyl ammonium chloride and NMGO-1 was changed to 1:0.3:0.05:0.0005 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing (i.e., NYKWSR-8) with a mesh size ≥80.
[0109] The viscosity average molecular weight of NYKWSR-8 obtained in Example 23 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 6.19 million Daltons.
[0110] Example 24: The method of Example 16 is followed, except that the associative monomer containing unsaturated double bonds and amphiphilic groups is replaced with N-tetradecyl substituted polyacrylamide to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing with a mesh size ≥ 80 mesh (i.e., NYKWSR-9).
[0111] The viscosity average molecular weight of NYKWSR-9 obtained in Example 24 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 14.16 million Daltons.
[0112] Example 25: The method of Example 23 was followed, except that the associative monomer was changed to N-tetradecyl substituted polyacrylamide to obtain a high-salt and high-temperature resistant instant associative thickener (i.e., NYKWSR-10) for fracturing with a mesh size of ≥80 mesh. The viscosity average molecular weight of NYKWSR-10 obtained in Example 25 was measured to be 5 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Molecular Weight Determination of Polyacrylamide".
[0113] The viscosity average molecular weight of NYKWSR-10 obtained in Example 25 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 5 million Daltons.
[0114] Example 26: The method of Example 16 is followed, except that the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is replaced with NMGO-2 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing with a mesh size ≥ 80 (i.e., NYKWSR-11).
[0115] The viscosity average molecular weight of NYKWSR-11 obtained in Example 26 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 15 million Daltons.
[0116] Example 27: The method of Example 23 is followed, except that the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is replaced with NMGO-2 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing with a mesh size ≥ 80 (i.e., NYKWSR-12).
[0117] The viscosity average molecular weight of NYKWSR-12 obtained in Example 27 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 7.1 million Daltons.
[0118] Example 28: The method of Example 24 is followed, except that the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is replaced with NMGO-2 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing with a mesh size ≥ 80 (i.e., NYKWSR-13).
[0119] The viscosity average molecular weight of NYKWSR-13 obtained in Example 28 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 14.67 million Daltons.
[0120] Example 29: The method of Example 25 is followed, except that the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is replaced with NMGO-2 to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing with a mesh size ≥ 80 (i.e., NYKWSR-14).
[0121] The viscosity average molecular weight of NYKWSR-14 obtained in Example 29 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 6.03 million Daltons.
[0122] Comparative Example 1: The method of Example 16 was followed, except that the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group was not added to obtain a heat-resistant and salt-resistant thickener for fracturing with a mesh size of ≥80 mesh (ie, DNYKWSR-1).
[0123] The viscosity average molecular weight of DNYKWSR-1 obtained in Comparative Example 1 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 16.4 million Daltons.
[0124] Comparative Example 2: The method of Example 23 was followed, except that the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group was not added to obtain a heat-resistant and salt-resistant thickener for fracturing with a mesh size of ≥80 mesh (i.e., DNYKWSR-2).
[0125] The viscosity average molecular weight of DNYKWSR-2 obtained in Comparative Example 2 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 8.56 million Daltons.
[0126] Comparative Example 3: The method of Example 24 was followed, except that the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group was not added to obtain a heat-resistant and salt-resistant thickener for fracturing with a mesh size of ≥80 mesh (i.e., DNYKWSR-3).
[0127] The viscosity average molecular weight of DNYKWSR-3 obtained in Comparative Example 3 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 15.8 million Daltons.
[0128] Comparative Example 4: The method of Example 25 was followed, except that the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group was not added to obtain a heat-resistant and salt-resistant thickener for fracturing with a mesh size of ≥80 mesh (i.e., DNYKWSR-4).
[0129] The viscosity average molecular weight of DNYKWSR-4 obtained in Comparative Example 4 was measured using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard "GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide" to be 7.95 million Daltons.
[0130] The performance test method of the high-salt and high-temperature resistant instant associative thickener for fracturing obtained in Examples 16 to 29 of the present invention is as follows:
[0131] (1) Adhesion time
[0132] Accurately weigh the calculated amount of thickener dry powder ≥80 mesh into a 500mL beaker pre-filled with an appropriate amount of brine (total mineralization 150000 mg / L, including calcium and magnesium ion content 15000 mg / L), stir and dissolve it with a high-speed stirrer at room temperature at a speed of 400±50 rad / min, use a glass rod to pick up the wire drawing, and record the corresponding time as the sticking time.
[0133] (2) Viscosity and viscosity release rate
[0134] A fixed amount of thickener powder was prepared into a 0.2% to 1.5% saline solution according to the method in (1). The solution was measured using a six-speed rotary viscometer at 100 r / min (170 s -1 ) to test the viscosity values at different dissolution times, and calculate the viscosity release rate according to the following formula. When the viscosity is lower than 10mPa·s, use a capillary viscometer to test the kinematic viscosity of the product.
[0135]
[0136] In the formula, V R is the real-time viscosity before stabilization, mPa·s; V F is the final stable viscosity, mPa·s; R V is the viscosity release rate, %.
[0137] (3) Heat resistance and shear resistance
[0138] RS6000 advanced rheometer PZ38 coaxial cylindrical rotor system was used at 180℃ and 170s -1 A 1.5% thickener saline solution was subjected to a temperature and shear resistance test, and the viscosity change curve over time and the final stable viscosity value were recorded. The duration from heating to the end of the test was 2 hours.
[0139] (4) Thixotropic energy
[0140] The thixotropy of 1.5% thickener salt solution was tested using a Physica MCR301 advanced rheometer in rotation mode at 180°C. -1 Up to 500s -1 Test from low shear to high shear within the shear rate range (stage 1, the obtained curve is an upward curve), 500s -1 Constant shear test 1min (2 stages), 500s -1 To 0.01s -1From high shear to low shear test (3 stages, the obtained curve is a downward curve), the hysteresis area A of the thixotropic loop composed of the upward curve and the downward curve of the shear stress changing with the shear rate is calculated by the Hysteresis Area I model, and the thixotropic energy is obtained.
[0141] The high-salt and high-temperature resistant instant associative thickeners for fracturing prepared in Examples 16 to 29 and the heat-resistant and salt-resistant thickeners for fracturing prepared in Comparative Examples 1 to 4 were tested by the above method at different concentrations at a mineralization degree of 150,000 mg / L (calcium and magnesium ion content of 15,000 mg / L). The results are shown in Table 1.
[0142] The high-salt-resistant and high-temperature-resistant instant associative thickener for fracturing prepared in Example 23 of the present invention with a concentration of 1.5% was compared with the heat-resistant and salt-resistant thickener for fracturing prepared in Comparative Example 2. The results are as follows: Figure 2 As shown;
[0143] The heat resistance and shear resistance of the high-salt and high-temperature resistant instant associative thickener for fracturing prepared in Example 25 of the present invention with a concentration of 1.5% were compared with the heat-resistant and salt-resistant thickener for fracturing prepared in Comparative Example 4. The results are as follows: Figure 3 shown.
[0144] The thixotropic energy of the high-salt-resistant and high-temperature-resistant instant associative thickener for fracturing prepared in Examples 23 and 25 of the present invention at a concentration of 1.5% is compared with that of the heat-resistant and salt-resistant thickener for fracturing prepared in Comparative Examples 2 and 4. The results are as follows: Figure 4 shown.
[0145] Depend on Figure 2 and Figure 4 It can be seen that in Example 23, hexadecyldimethylallylammonium chloride is used as an associative monomer containing unsaturated double bonds and amphiphilic groups, and a polymerizable modified graphene oxide containing both sulfonic acid groups and hydroxyl groups is introduced. The resulting high-salt and high-temperature resistant instant associative thickener for fracturing (NYKWSR-8) has a temperature-resistant and shear-resistant stable viscosity that is 12 mPa·s higher than that of the temperature-resistant and salt-resistant thickener for fracturing obtained in Comparative Example 2 (without the introduction of NMGO-1) at a concentration of 1.5%, and a thixotropic energy that is 175 Pa / s higher.
[0146] From Figure 3 and Figure 4It can also be seen that after the associative monomer containing unsaturated double bonds and amphiphilic groups is replaced with N-tetradecyl substituted polyacrylamide in Example 25, the obtained high-salt and high-temperature resistant instant associative thickener for fracturing (NYKWSR-10) has a temperature-resistant and shear-resistant stable viscosity that is 9 mPa·s higher than that of the temperature-resistant and salt-resistant thickener for fracturing obtained in Comparative Example 4 (without the introduction of NMGO-1) at a dosage of 1.5%, and the thixotropic energy is 155 Pa / s higher.
[0147] Therefore, it can be seen that the salt resistance, temperature resistance and rapid solubility of the high-salt and high-temperature resistant fast-dissolving associative thickener for fracturing obtained by introducing the polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups are greatly improved.
[0148] In summary, the present invention introduces a monomer containing a salt-resistant sulfonic acid group, a high-temperature resistant two-dimensional planar structure, and a strong hydrophilic group into the macromolecular skeleton of the associative thickener, thereby simultaneously improving the high salt resistance, high temperature resistance, and quick dissolution properties of the associative thickener.
[0149] Table 1
[0150] .
[0151] The above technical features constitute the embodiments of the present invention, which have strong adaptability and implementation effect. Non-essential technical features can be added or reduced according to actual needs to meet the requirements of different situations.
Claims
1. A high-salt and high-temperature resistant instant associative thickener for fracturing, characterized in that The raw materials include acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups, wherein the mass ratio of acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups is: 1:0.15 to 0.3:0.005 to 0.05:0.00005 to 0.0005, the associative monomer containing unsaturated double bonds and amphiphilic groups is one or more of long-chain alkyl unsaturated quaternary ammonium salt and N-alkyl substituted acrylamide associative monomer, The structural formula of the associative monomer containing an unsaturated double bond and an amphiphilic group is: , The structural formula of R1 is: 、 One of wherein m is an integer from 11 to 19, n is an integer from 0 to 4, and z is an integer from 1 to 2, The structural formula of R2 is: or , Here, n is an integer from 11 to 19.
2. The high-salt and high-temperature resistant instant associative thickener for fracturing according to claim 1, characterized in that The structural formula of the polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is: , The structural formula of R3 is: , Wherein, n is an integer from 0 to 1, The structural formula of R4 is: , Here, n is an integer from 0 to 1.
3. The high-salt and high-temperature resistant instant associative thickener for fracturing according to claim 1 or 2, characterized in that The polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group is obtained according to the following method: The first step is to ultrasonically disperse the required amount of graphene oxide with an ethanol aqueous solution having a mass concentration of 90% to 95%, add the required amount of a silane coupling agent containing an unsaturated double bond at 55° C. to 65° C. and continuously stir, and reflux for 6 h to 8 h to obtain a first reaction mixture; The second step is to cool the reaction mixture to room temperature overnight, vacuum filter and wash twice with acetone, and dry at 50° C. to 70° C. for 17 to 18 hours to obtain a modified graphene oxide intermediate containing unsaturated double bonds; The third step is to ultrasonically treat the required amount of the modified graphene oxide intermediate with unsaturated double bonds in deionized water for 1.5 to 2.5 hours to obtain a uniform intermediate dispersion; Step 4: dissolving the required amount of 6-amino-4-hydroxy-2-naphthalenesulfonate in deionized water pre-added with 0.2 mL to 0.5 mL of aqueous ammonia, and then adding it to the intermediate dispersion under continuous stirring, and refluxing at 70° C. to 80° C. for 8 h to 9 h to obtain a second reaction mixture; The fifth step is to cool the second reaction mixture to room temperature and stand it for 8 hours, centrifuge it at 1200r / min in a high-speed centrifuge for 15 to 20 minutes, separate the upper liquid, and wash the upper liquid three times with 60% to 70% ethanol aqueous solution and pure water to obtain a polymerizable modified graphene oxide functional monomer containing sulfonic acid group and hydroxyl group.
4. The high-salt and high-temperature resistant instant associative thickener for fracturing according to claim 3, characterized in that In the first step, the mass ratio of graphene oxide to the silane coupling agent containing unsaturated double bonds is 1:1.5 to 2, and the silane coupling agent containing unsaturated double bonds is one or more of vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, and allyltriethoxysilane.
5. The high-salt and high-temperature resistant instant associative thickener for fracturing according to claim 3 or 4, characterized in that In the fourth step, the molar concentration of ammonia water is 1 mol / L, and the mass ratio of the modified graphene oxide intermediate containing unsaturated double bonds to 6-amino-4-hydroxy-2-naphthalenesulfonate is 1:2 to 3.
6. The high-salt and high-temperature resistant instant associative thickener for fracturing according to any one of claims 1 to 5, characterized in that Obtained as follows: S1, mixing and dissolving required amounts of acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups in water to obtain a mixed solution with a mass concentration of 18% to 28%; S2, adjusting the pH value of the mixed solution to 7 to 8 with a pH adjuster, refrigerating the mixed solution for 30 minutes to lower the temperature to -5°C, and then adding a required amount of a low-temperature composite initiator to initiate a polymerization reaction to obtain a colloidal product; S3, chopping, sieving and drying the colloidal product to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing.
7. The high-salt and high-temperature resistant instant associative thickener for fracturing according to claim 6, characterized in that In step S2, the pH adjuster is one or more of sodium bicarbonate, sodium hydroxide, potassium hydroxide, citric acid, and glacial acetic acid, the low-temperature composite initiator is a mixture of sodium persulfate, sodium bisulfite and an inorganic compound oxidant in a volume ratio of 1:1:0.1, the volume ratio of the low-temperature composite initiator to the mixed solution is 1:250, and the polymerization reaction temperature is -5°C to 20°C, wherein the inorganic compound oxidant is one or more of ammonium cerium nitrate and ammonium cerium sulfate.
8. A method for preparing a high-salt-resistant and high-temperature-resistant instant associative thickener for fracturing according to claim 1, 2, 3, 4, 5, or 7, characterized in that Proceed as follows: S1, mixing and dissolving required amounts of acrylamide hydrophilic monomer, sodium acrylate hydrophilic monomer, associative monomer containing unsaturated double bonds and amphiphilic groups, and polymerizable modified graphene oxide functional monomer containing sulfonic acid groups and hydroxyl groups in water to obtain a mixed solution with a mass concentration of 18% to 28%; S2, adjusting the pH value of the mixed solution to 7 to 8 with a pH regulator, refrigerating the mixed solution for 30 minutes to reduce the temperature of the mixed solution to -5°C, and then adding a required amount of a low-temperature composite initiator to initiate a polymerization reaction to obtain a colloidal product, wherein the pH regulator is one or more of sodium bicarbonate, sodium hydroxide, potassium hydroxide, citric acid, and glacial acetic acid, the low-temperature composite initiator is a mixture of sodium persulfate, sodium bisulfite and an inorganic compound oxidant in a volume ratio of 1:1:0.1, the volume ratio of the low-temperature composite initiator to the mixed solution is 1:250, the polymerization reaction temperature is -5°C to 20°C, and the inorganic compound oxidant is one or more of ammonium cerium nitrate and ammonium cerium sulfate; S3, chopping, sieving and drying the colloidal product to obtain a high-salt and high-temperature resistant instant associative thickener for fracturing.
Citation Information
Patent Citations
A fast-dissolving polyacrylamide and its preparation method
CN105085801B
Temperature-resistant and salt-resistant fast-dissolving thickener for seawater-based fracturing fluids and its preparation method
CN106190088B
Slickwater system considering both drag reduction and sand carrying and preparation method thereof
CN111635749A
A kind of heat-resistant and salt-resistant quick-dissolving polymer for oil displacement and preparation method thereof
CN114716606B
A temperature- and salt-resistant, fast-dissolving polyacrylamide, its preparation method, and its applications.
CN115947891B