A FRP composite material and its preparation method and application

By using components such as vinyl ester resin, epoxy resin, fluorinated silicone and triphenyltin chloride in FRP composite materials, the water resistance, corrosion resistance and microbial resistance of traditional FRP composite materials in aqueous environments are solved. The problem of insufficient performance is achieved by achieving higher water resistance and anti-microbial properties and extending the service life.

CN118496627BActive Publication Date: 2024-10-22YIZHENG ZHONGZHI COMPOSITE MATERIAL PROD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410953999.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-22
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Traditional FRP composite materials are difficult to meet the requirements for high water resistance, corrosion resistance, and microbial resistance in environments such as rivers, pools, and oceans, resulting in a short service life in these environments.

Method used

Using components such as vinyl ester resin, epoxy resin, fluorine-containing silicone, triphenyltin chloride and organic guanidine compounds, through copolymerization and specific proportions, it forms a product with high water resistance, corrosion resistance and Antimicrobial properties of FRP composites.

Benefits of technology

It significantly improves the water resistance, corrosion resistance and anti-microbial properties of FRP composite materials, prolongs its service life, and especially shows better stability and resistance to crack expansion in low-temperature water environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a FRP composite material and a preparation method and application thereof, and relates to the technical field of fiber reinforced materials. The FRP composite material includes the following components in parts by weight: 30-50 parts of vinyl ester resin, 40-60 parts of epoxy resin, 2-5 parts of fluorinated organosilicon, 2-4 parts of triphenyltin chloride, 1-3 parts of organic guanidine compounds, 1-3 parts of coupling agents, 1-3 parts of antioxidants, and 15-30 parts of reinforcing fibers. The present application adopts vinyl ester resin, epoxy resin, fluorinated organosilicon, triphenyltin chloride and organic guanidine compounds, and through the joint action of each component, the water resistance, corrosion resistance and microbial resistance of the FRP composite material can be improved, the erosion of the FRP composite material by moisture, salt and microorganisms can be reduced, and the service life of the FRP composite material can be extended.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fiber reinforced materials, and in particular to a FRP composite material and a preparation method and application thereof. Background Art

[0002] FRP (fiber reinforced material) composite material is a composite material formed by winding, molding or pultrusion of reinforcing fiber materials, such as glass fiber, carbon fiber, aramid fiber, etc., and matrix materials.

[0003] In the related art, a FRP profile composite material is disclosed, which is made of the following raw materials in parts by weight: 70-80 parts of functional resin, 1-3 parts of epoxy-containing polysiloxane hyperbranched polymer, 5-8 parts of amino-terminated hyperbranched polybenzimidazole, 1-2 parts of coupling agent, 0.3-0.6 parts of antioxidant, 5-10 parts of nano boron fiber, and 10-20 parts of glass fiber; the functional resin is made of N-acryloylmorpholine, 2-(2-(vinyloxy)ethyl)isoindoline-1,3-dione, N-(4-cyano-3-trifluoromethylphenyl)methacrylamide, and 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione through free radical copolymerization. The above-mentioned FRP profile composite materials have sufficient aging resistance, excellent mechanical strength and fatigue resistance, and have been widely used in the fields of construction, transportation, environmental protection, etc.

[0004] However, the application of FRP composite materials in rivers, pools, oceans and other environments has put forward higher requirements for the water resistance, corrosion resistance and microbial resistance of FRP composite materials. Traditional FRP composite materials have certain shortcomings in these aspects and are difficult to meet the growing demand.

[0005] Therefore, how to prepare an FRP composite material with high water resistance, corrosion resistance and microbial resistance has become a problem that needs to be solved urgently. Summary of the invention

[0006] In order to improve the water resistance, corrosion resistance and microbial resistance of FRP composite materials, the present application provides an FRP composite material and a preparation method and application thereof.

[0007] In a first aspect, the present application provides a FRP composite material, which adopts the following technical solution:

[0008] A FRP composite material comprises the following components in parts by weight: 30-50 parts of vinyl ester resin, 40-60 parts of epoxy resin, 2-5 parts of fluorine-containing silicone, 2-4 parts of triphenyltin chloride, 1-3 parts of organic guanidine compounds, 1-3 parts of coupling agents, 1-3 parts of antioxidants and 15-30 parts of reinforcing fibers.

[0009] By adopting the above technical solution, vinyl ester resin can effectively resist the penetration and erosion of water. Epoxy resin has strong bonding force and chemical corrosion resistance, which enhances the overall stability of the composite material. Fluorine-containing silicone has extremely low surface energy, making it difficult for moisture and microorganisms to adhere. The present application has found through experiments that the water resistance of the composite material can be improved by compounding the vinyl ester resin, epoxy resin and fluorine-containing silicone in the above ratio.

[0010] Moreover, the present application adopts triphenyltin chloride and organic guanidine compounds, triphenyltin chloride can react with hydroxyl groups in the resin to form a stable anticorrosion layer on the surface of the composite material, and the organic guanidine compounds are dispersed in the composite material. When microorganisms attach to the surface of the composite material, the anticorrosion layer formed by triphenyltin chloride can destroy the cell structure of the microorganisms, and the organic guanidine compounds can interfere with the metabolic process of the microorganisms, thereby inhibiting the growth and reproduction of microorganisms, and effectively preventing the corrosion of the composite material by microorganisms. The two work together to provide a strong antimicrobial protection for the composite material.

[0011] Therefore, the present application adopts the above-mentioned technical scheme to improve the water resistance, corrosion resistance and microbial resistance of the FRP composite material. When the FRP composite material of the present application is used in aquaculture ponds, rivers or oceans and other environments, it can reduce the erosion of the FRP composite material by moisture, salt and microorganisms, and extend the service life of the FRP composite material.

[0012] In a specific embodiment, the fluorine-containing silicone is a polysiloxane containing a perfluoroalkyl chain in the side chain structure.

[0013] By adopting the above technical solution, the perfluoroalkyl chain is introduced into the side chain structure of polysiloxane, which can give the fluorinated silicone a lower surface energy, thereby further enhancing the anti-adhesion, self-cleaning and other properties of the FRP composite material, so that the FRP composite material can remain stable under more harsh environmental conditions.

[0014] In a specific embodiment, the perfluoroalkyl chain is any one of a perfluorobutyl chain, a perfluorohexyl chain or a perfluorooctyl chain.

[0015] By adopting the above technical solution, the present application has experimentally found that by introducing perfluorobutane chains, perfluorohexane chains or perfluorooctane chains into the side-linked structure of fluorinated silicone, the flexibility and low-temperature elasticity of FRP composite materials can be improved, so that FRP composite materials can be applied to adapt to low-temperature water environments such as aquaculture ponds, rivers and oceans. This may be because perfluoroalkyl chains with shorter carbon chain lengths can improve the low-temperature resistance of FRP composite materials.

[0016] In a specific embodiment, the organic guanidine compound is at least one of 1,3-diaminoguanidine hydrochloride, (2-methyl-5-nitrophenyl)guanidine nitrate, and diethylguanidine sulfate.

[0017] By adopting the above technical scheme, 1,3-diaminoguanidine hydrochloride has excellent antibacterial properties. When combined with triphenyltin chloride, it can form a powerful antibacterial synergistic system, significantly enhancing the antibacterial effect of the composite material. The amino group in the molecular structure of 1,3-diaminoguanidine hydrochloride can form hydrogen bonds with the resin, thereby improving the compatibility with the resin, ensuring that the composite material has excellent physical properties while maintaining antibacterial properties. (2-methyl-5-nitrophenyl)guanidine nitrate is an efficient and stable antibacterial agent. When used together with triphenyltin chloride, it can produce a synergistic antibacterial effect and effectively inhibit the growth of a variety of microorganisms. The methyl group of (2-methyl-5-nitrophenyl)guanidine nitrate helps to enhance compatibility with the resin, reduce interfacial tension, and make the composite material more uniform and stable. Diethylguanidine sulfate has excellent antibacterial properties. When combined with triphenyltin chloride, it can significantly enhance the antibacterial ability of the composite material. The introduction of the ethyl group helps to improve the compatibility with the resin, so that the composite material has good processing performance and mechanical properties while maintaining the antibacterial effect.

[0018] In a specific embodiment, the organic guanidine compound is (2-methyl-5-nitrophenyl)guanidine nitrate.

[0019] By adopting the above technical solution, the present applicant has found through experiments that, compared with other organic guanidine compounds, the use of (2-methyl-5-nitrophenyl)guanidine nitrate can help further improve the antibacterial properties and physical properties of the composite material.

[0020] In a specific embodiment, the epoxy resin is a mixture of bisphenol A epoxy resin and flexible aliphatic epoxy resin in a weight ratio of 1: (0.6-1.5).

[0021] By adopting the above technical scheme, bisphenol A type epoxy resin has excellent mechanical properties and chemical corrosion resistance, which can ensure that the composite material maintains stable performance in harsh environments. The hydroxyl and ether bonds in its molecular structure help to improve the compatibility with organic guanidine compounds and triphenyltin chloride, forming a uniformly dispersed composite material system. Flexible aliphatic epoxy resin has good toughness and impact resistance, which can enhance the composite material's resistance to crack propagation. Its lower viscosity helps to better infiltrate and wrap the antibacterial agent, thereby improving the dispersion effect of the antibacterial agent in the composite material. The present application adopts a mixture of the two epoxy resins in the above weight ratio, which can further improve the antibacterial properties and physical properties of the composite material.

[0022] In a specific embodiment, the reinforcing fiber includes at least one of glass fiber, carbon fiber or basalt fiber.

[0023] By adopting the above technical solution, the present applicant has found that by selecting any of the above fibers, an FRP composite material with excellent physical properties, water resistance and microbial resistance can be obtained.

[0024] In a specific embodiment, the reinforcing fiber is a mixture of basalt fiber and glass fiber in a weight ratio of 1: (0.4-0.7).

[0025] By adopting the above technical solution, the present applicant has found through experiments that using a mixture of basalt fiber and glass fiber within the above ratio range as reinforcing fiber can help further improve the physical properties of the FRP composite material, which helps to extend the service life of the FRP composite material.

[0026] In a second aspect, the present application provides a method for preparing a FRP composite material, which adopts the following technical solution:

[0027] A method for preparing a FRP composite material comprises the following steps:

[0028] Premixing: Evenly mix the vinyl ester resin, epoxy resin, fluorinated silicone, triphenyltin chloride and organic guanidine compound to obtain a mixture A; evenly mix the coupling agent, antioxidant and reinforcing fiber to obtain a mixture B;

[0029] Molding: Mix mixture A and mixture B evenly to obtain mixture C, pour mixture C into a mold, discharge bubbles in mixture C, place the mold at 82-88°C, heat for 2.2-2.6h, then place it at 135-142°C, heat for 3-4h, end heating, cool and demold to obtain an FRP composite material.

[0030] By adopting the above technical scheme, the method first prepares mixture A and mixture B, which helps to evenly disperse fluorinated silicone, triphenyltin chloride and organic guanidine compounds in the resin. In the molding step, the heating temperature and time are controlled within the above range, which helps to improve the molding effect and obtain an FRP composite material with good physical properties, water resistance and microbial resistance.

[0031] In a third aspect, the present application provides an application of an FRP composite material, using the following technical solution:

[0032] The invention discloses an application of an FRP composite material in an aquaculture pond. The FRP composite material is used to prepare any structure or component in the aquaculture pond.

[0033] In summary, the present application includes at least one of the following beneficial technical effects:

[0034] The present application adopts vinyl ester resin, epoxy resin, fluorinated silicone, triphenyltin chloride and organic guanidine compounds, and through the joint action of each component, the water resistance, corrosion resistance and microbial resistance of the FRP composite material can be improved, the erosion of the FRP composite material by moisture, salt and microorganisms can be reduced, and the service life of the FRP composite material can be extended;

[0035] The present application helps to further improve the water resistance, corrosion resistance and microbial resistance of FRP composite materials in low-temperature water environments by using polysiloxane containing perfluorobutane chains, perfluorohexane chains or perfluorooctane chains in the side chain structure;

[0036] The present application improves the compatibility with the resin by using 1,3-diaminoguanidine hydrochloride, (2-methyl-5-nitrophenyl)guanidine nitrate or diethylguanidine sulfate as the organic guanidine compound, ensuring that the composite material has excellent physical properties while maintaining antibacterial properties. DETAILED DESCRIPTION

[0037] The present application is further described in detail below in combination with preparation examples, embodiments and comparative examples.

[0038] Preparation example of fluorinated silicone

[0039] Preparation Example 1

[0040] This preparation example provides a fluorine-containing organosilicon, using the following raw materials: 850 g of dimethylstyrylsilane, 600 g of perfluorobutylethyltriethoxysilane, 7.80 g of tris(pentafluorophenyl)borane, and 2200 g of toluene.

[0041] Toluene was divided into two equal parts. Under a nitrogen atmosphere, dimethylstyrylsilane was dissolved in the first part of toluene to obtain solution A. Perfluorobutylethyltriethoxysilane and tris(pentafluorophenyl)borane were dissolved in the second part of toluene to obtain solution B.

[0042] At room temperature, solution B was added dropwise to solution A. When H2 began to be released, stirring was continued at room temperature, and the content of dimethylstyrylsilane in the reaction system was continuously detected. When the content of dimethylstyrylsilane was 0, toluene was removed under reduced pressure, and petroleum ether (PE) was used as an eluent, and the crude product was purified by silica gel column chromatography (Rf=0.3) to obtain a polysiloxane fluorinated silicone with a side chain structure of a perfluorobutyl chain.

[0043] Preparation Example 2

[0044] This preparation example provides a fluorine-containing organosilicon. The only difference between this preparation example and preparation example 1 is that perfluorobutylethyltriethoxysilane is replaced with an equal amount of perfluorohexyltriethoxysilane, and finally a polysiloxane having a side chain structure of a perfluorohexyl chain is obtained.

[0045] Preparation Example 3

[0046] This preparation example provides a fluorine-containing silicone. The only difference between this preparation example and Preparation Example 1 is that an equal amount of perfluorooctyltriethoxysilane is used to replace perfluorobutylethyltriethoxysilane, and finally a polysiloxane having a side chain structure of a perfluorooctyl chain is obtained.

[0047] Preparation Example 4

[0048] This preparation example provides a fluorine-containing organosilicon. The only difference between this preparation example and preparation example 1 is that perfluorobutylethyltriethoxysilane is replaced with an equal amount of perfluorodecyltriethoxysilane, and finally a polysiloxane having a side chain structure of a perfluorodecyl chain is obtained. Example

[0049] Example 1

[0050] This embodiment provides an FRP composite material, using the following raw materials: 400g epoxy vinyl ester resin (brand: 901), 250g bisphenol A epoxy resin (brand: NPEL-12), 250g flexible aliphatic epoxy resin (model: XZ 9246692465), 35g fluorine-containing silicone prepared in Preparation Example 1, 30g triphenyltin chloride, 20g 1,3-diaminoguanidine hydrochloride, 20g silane coupling agent (KH560), 20g antioxidant (1076), 220g alkali-free chopped glass fiber. The single filament diameter of the alkali-free chopped glass fiber is 11 microns and the length is 4 mm.

[0051] The present application also provides a method for preparing a FRP composite material, which comprises the following steps:

[0052] Epoxy vinyl ester resin, bisphenol A epoxy resin, flexible aliphatic epoxy resin, fluorinated silicone, triphenyltin chloride and 1,3-diaminoguanidine hydrochloride are mixed uniformly to obtain a mixture A; a silane coupling agent, an antioxidant and alkali-free chopped glass fibers are mixed uniformly to obtain a mixture B;

[0053] Mixture A and mixture B are mixed evenly to obtain mixture C, and mixture C is poured into a mold. The mold is then placed in a vacuum drying oven and vacuumed for 2 hours to remove bubbles in mixture C. The mold is then placed at 84°C and kept warm for 2.4 hours. The temperature is then raised to 137°C and kept warm for 3.5 hours. The heating is terminated, and the mold is demolded after natural cooling to obtain an FRP composite material.

[0054] Example 2

[0055] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the FRP composite material adopts the following raw materials: 400g epoxy vinyl ester resin (brand: 901), 250g bisphenol A epoxy resin (brand: NPEL-12), 250g flexible aliphatic epoxy resin (model: XZ 92466 92465), 20g fluorine-containing silicone prepared in the preparation example 1, 20g triphenyltin chloride, 10g 1,3-diaminoguanidine hydrochloride, 10g silane coupling agent (KH560), 10g antioxidant (1076), and 150g alkali-free chopped glass fiber.

[0056] Example 3

[0057] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the FRP composite material uses the following raw materials: 400 g of epoxy vinyl ester resin (brand: 901), 250 g of bisphenol A epoxy resin (brand: NPEL-12), 250 g of flexible aliphatic epoxy resin (model: XZ 92466 92465), 50 g of fluorine-containing silicone prepared in the preparation example 1, 40 g of triphenyltin chloride, 30 g of 1,3-diaminoguanidine hydrochloride, 30 g of silane coupling agent (KH560), 30 g of antioxidant (1076), and 300 g of alkali-free chopped glass fiber.

[0058] Example 4

[0059] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the FRP composite material uses the following raw materials: 300 g of epoxy vinyl ester resin (brand: 901), 300 g of bisphenol A epoxy resin (brand: NPEL-12), 300 g of flexible aliphatic epoxy resin (model: XZ 92466 92465), 35 g of fluorine-containing silicone prepared in the preparation example 1, 30 g of triphenyltin chloride, 20 g of 1,3-diaminoguanidine hydrochloride, 20 g of silane coupling agent (KH560), 20 g of antioxidant (1076), and 220 g of alkali-free chopped glass fiber.

[0060] Example 5

[0061] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the FRP composite material uses the following raw materials: 500 g of epoxy vinyl ester resin (brand: 901), 200 g of bisphenol A epoxy resin (brand: NPEL-12), 200 g of flexible aliphatic epoxy resin (model: XZ 92466 92465), 35 g of fluorine-containing silicone prepared in Preparation Example 1, 30 g of triphenyltin chloride, 20 g of 1,3-diaminoguanidine hydrochloride, 20 g of silane coupling agent (KH560), 20 g of antioxidant (1076), and 220 g of alkali-free chopped glass fiber.

[0062] Example 6

[0063] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the FRP composite material uses the following raw materials: 400 g of epoxy vinyl ester resin (brand: 901), 312.5 g of bisphenol A epoxy resin (brand: NPEL-12), 187.5 g of flexible aliphatic epoxy resin (model: XZ 92466 92465), 35 g of fluorine-containing silicone prepared in the preparation example 1, 30 g of triphenyltin chloride, 20 g of 1,3-diaminoguanidine hydrochloride, 20 g of silane coupling agent (KH560), 20 g of antioxidant (1076), and 220 g of alkali-free chopped glass fiber.

[0064] Example 7

[0065] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the FRP composite material uses the following raw materials: 400 g of epoxy vinyl ester resin (brand: 901), 200 g of bisphenol A epoxy resin (brand: NPEL-12), 300 g of flexible aliphatic epoxy resin (model: XZ 92466 92465), 35 g of fluorine-containing silicone prepared in the preparation example 1, 30 g of triphenyltin chloride, 20 g of 1,3-diaminoguanidine hydrochloride, 20 g of silane coupling agent (KH560), 20 g of antioxidant (1076), and 220 g of alkali-free chopped glass fiber.

[0066] Example 8

[0067] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the FRP composite material uses the following raw materials: 400 g of epoxy vinyl ester resin (brand: 901), 333 g of bisphenol A epoxy resin (brand: NPEL-12), 167 g of flexible aliphatic epoxy resin (model: XZ 92466 92465), 35 g of fluorine-containing silicone prepared in the preparation example 1, 30 g of triphenyltin chloride, 20 g of 1,3-diaminoguanidine hydrochloride, 20 g of silane coupling agent (KH560), 20 g of antioxidant (1076), and 220 g of alkali-free chopped glass fiber.

[0068] Example 9

[0069] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the FRP composite material uses the following raw materials: 400 g of epoxy vinyl ester resin (brand: 901), 190 g of bisphenol A epoxy resin (brand: NPEL-12), 310 g of flexible aliphatic epoxy resin (model: XZ 92466 92465), 35 g of fluorine-containing silicone prepared in the preparation example 1, 30 g of triphenyltin chloride, 20 g of 1,3-diaminoguanidine hydrochloride, 20 g of silane coupling agent (KH560), 20 g of antioxidant (1076), and 220 g of alkali-free chopped glass fiber.

[0070] Example 10

[0071] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the FRP composite material uses the following raw materials: 400 g of epoxy vinyl ester resin (brand: 901), 500 g of bisphenol A epoxy resin (brand: NPEL-12), 35 g of fluorine-containing silicone prepared in the preparation example 1, 30 g of triphenyltin chloride, 20 g of 1,3-diaminoguanidine hydrochloride, 20 g of silane coupling agent (KH560), 20 g of antioxidant (1076), and 220 g of alkali-free chopped glass fiber.

[0072] Embodiment 11

[0073] This embodiment provides an FRP composite material. The only difference between this embodiment and Embodiment 1 is that an equal amount of chopped carbon fibers is used to replace the alkali-free chopped glass fibers. The single fiber diameter of the chopped carbon fibers is 11 microns and the length is 4 millimeters.

[0074] Example 12

[0075] This embodiment provides an FRP composite material. The only difference between this embodiment and Embodiment 1 is that an equal amount of chopped basalt fibers are used to replace the alkali-free chopped glass fibers. The single filament diameter of the chopped basalt fibers is 11 microns and the length is 4 millimeters.

[0076] Embodiment 13

[0077] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the alkali-free chopped glass fiber is replaced by a mixture of equal amounts of chopped carbon fiber and alkali-free chopped glass fiber in a weight ratio of 1:0.5, and the single fiber diameter of the chopped carbon fiber is 11 microns and the length is 4 mm.

[0078] Embodiment 14

[0079] This embodiment provides an FRP composite material. The only difference between this embodiment and Example 1 is that the alkali-free chopped glass fiber is replaced by a mixture of equal amounts of chopped basalt fibers and alkali-free chopped glass fibers in a weight ratio of 1:0.5, and the single fiber diameter of the chopped basalt fibers is 11 microns and the length is 4 mm.

[0080] Embodiment 15

[0081] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the alkali-free chopped glass fiber is replaced by a mixture of equal amounts of chopped basalt fiber and chopped carbon fiber in a weight ratio of 1:0.5, and the single fiber diameters of the chopped basalt fiber and the chopped carbon fiber are both 11 microns and 4 mm in length.

[0082] Example 16

[0083] The present embodiment provides an FRP composite material. The only difference between the present embodiment and the embodiment 1 is that the alkali-free chopped glass fiber is replaced by a mixture of equal amounts of alkali-free chopped glass fiber, chopped basalt fiber and chopped carbon fiber in a weight ratio of 1:0.5:0.5, and the single fiber diameters of the chopped basalt fiber and the chopped carbon fiber are both 11 microns and 4 mm in length.

[0084] Embodiment 17

[0085] This embodiment provides an FRP composite material. The only difference between this embodiment and Embodiment 1 is that the alkali-free chopped glass fiber is replaced by a mixture of equal amounts of chopped basalt fiber and alkali-free chopped glass fiber in a weight ratio of 1:0.3, and the single fiber diameter of the chopped basalt fiber is 11 microns and the length is 4 mm.

[0086] Embodiment 18

[0087] This embodiment provides an FRP composite material. The only difference between this embodiment and Embodiment 1 is that the alkali-free chopped glass fiber is replaced by a mixture of equal amounts of chopped basalt fiber and alkali-free chopped glass fiber in a weight ratio of 1:0.4, and the single fiber diameter of the chopped basalt fiber is 11 microns and the length is 4 mm.

[0088] Embodiment 19

[0089] This embodiment provides an FRP composite material. The only difference between this embodiment and Example 1 is that the alkali-free chopped glass fiber is replaced by a mixture of equal amounts of chopped basalt fibers and alkali-free chopped glass fibers in a weight ratio of 1:0.7, and the single fiber diameter of the chopped basalt fibers is 11 microns and the length is 4 mm.

[0090] Embodiment 20

[0091] This embodiment provides an FRP composite material. The only difference between this embodiment and Example 1 is that the alkali-free chopped glass fiber is replaced by a mixture of equal amounts of chopped basalt fibers and alkali-free chopped glass fibers in a weight ratio of 1:0.8, and the single fiber diameter of the chopped basalt fibers is 11 microns and the length is 4 mm.

[0092] Embodiment 21

[0093] This embodiment provides a FRP composite material. The only difference between this embodiment and Embodiment 1 is that 1,3-diaminoguanidine hydrochloride is replaced by an equal amount of (2-methyl-5-nitrophenyl)guanidine nitrate.

[0094] Embodiment 22

[0095] This embodiment provides a FRP composite material. The only difference between this embodiment and Embodiment 1 is that an equal amount of diethylguanidine sulfate is used to replace 1,3-diaminoguanidine hydrochloride.

[0096] Embodiment 23

[0097] This embodiment provides a FRP composite material. The only difference between this embodiment and Example 1 is that the fluorinated organosilicon prepared in Preparation Example 1 is replaced by an equal amount of the fluorinated organosilicon prepared in Preparation Example 2.

[0098] Embodiment 24

[0099] This embodiment provides a FRP composite material. The only difference between this embodiment and Example 1 is that the fluorinated organosilicon prepared in Preparation Example 1 is replaced by an equal amount of the fluorinated organosilicon prepared in Preparation Example 3.

[0100] Embodiment 25

[0101] This embodiment provides a FRP composite material. The only difference between this embodiment and Example 1 is that the fluorinated organosilicon prepared in Preparation Example 1 is replaced by an equal amount of the fluorinated organosilicon prepared in Preparation Example 4.

[0102] Embodiment 26

[0103] This embodiment provides a FRP composite material. The difference between this embodiment and embodiment 1 is that the preparation method of the FRP composite material adopts the following steps:

[0104] Epoxy vinyl ester resin, bisphenol A epoxy resin, flexible aliphatic epoxy resin, fluorinated silicone, triphenyltin chloride and 1,3-diaminoguanidine hydrochloride are mixed uniformly to obtain a mixture A; a silane coupling agent, an antioxidant and alkali-free chopped glass fibers are mixed uniformly to obtain a mixture B;

[0105] Mixture A and mixture B are mixed evenly to obtain mixture C, and mixture C is poured into a mold. The mold is then placed in a vacuum drying oven and vacuumed for 2 hours to remove bubbles in mixture C. The mold is then placed at 82°C and kept warm for 2.6 hours. The temperature is then raised to 135°C and kept warm for 4 hours. The heating is terminated, and the mold is demolded after natural cooling to obtain an FRP composite material.

[0106] Embodiment 27

[0107] This embodiment provides a FRP composite material. The difference between this embodiment and embodiment 1 is that the preparation method of the FRP composite material adopts the following steps:

[0108] Epoxy vinyl ester resin, bisphenol A epoxy resin, flexible aliphatic epoxy resin, fluorinated silicone, triphenyltin chloride and 1,3-diaminoguanidine hydrochloride are mixed uniformly to obtain a mixture A; a silane coupling agent, an antioxidant and alkali-free chopped glass fibers are mixed uniformly to obtain a mixture B;

[0109] Mixture A and mixture B are mixed evenly to obtain mixture C, and mixture C is poured into a mold. The mold is then placed in a vacuum drying oven and vacuumed for 2 hours to remove bubbles in mixture C. The mold is then placed at 88°C and kept warm for 2.2 hours. The temperature is then raised to 142°C and kept warm for 3 hours. The heating is terminated, and the mold is demolded after natural cooling to obtain an FRP composite material. Comparative Example

[0110] Comparative Example 1

[0111] This comparative example provides a FRP composite material. The only difference between this comparative example and Example 1 is that the fluorine-containing silicone prepared in Preparation Example 1 is replaced by an equal amount of epoxy vinyl ester resin (brand: 901).

[0112] Comparative Example 2

[0113] This comparative example provides a FRP composite material. The difference between this comparative example and Example 1 is that an equal amount of epoxy vinyl ester resin (brand: 901) is used to replace triphenyltin chloride.

[0114] Comparative Example 3

[0115] This comparative example provides a FRP composite material. The only difference between this comparative example and Example 1 is that an equal amount of epoxy vinyl ester resin (brand: 901) is used to replace 1,3-diaminoguanidine hydrochloride.

[0116] Performance testing

[0117] The following performance tests were performed on the FRP composite materials provided in Examples 1-27 and Comparative Examples 1-3:

[0118] Bending strength: Tested in accordance with GBT1449-2005 “Test method for bending properties of fiber reinforced plastics”.

[0119] Tensile strength: Tested in accordance with GB / T1447-2005 “Test method for tensile properties of fiber reinforced plastics”.

[0120] Water resistance and corrosion resistance: According to ASTM D1141-98 (2003), artificial seawater was prepared with distilled water. The pH value of artificial seawater was adjusted to 8.0 with NaOH solution. Before the experiment, the surface of the FRP composite material sample was polished with sandpaper. The experimental corrosion method adopted full immersion corrosion. The ambient temperature of artificial seawater was 2±1℃ and 35±1℃. The test cycle was 1-4 months, and each corrosion cycle was separated by one month, for a total of four cycles. The corrosion surface morphology was observed at the end of each cycle. After the four cycles of corrosion test, the tensile strength and bending strength of the samples were tested respectively.

[0121] Microbial resistance: According to QB / T2591-2003A "Test Methods and Antibacterial Effects of Antibacterial Plastics", the antibacterial test of FRP composite material samples was carried out. The test bacteria: Escherichia coli ATCC25922, Staphylococcus aureus ATCC6538.

[0122] The above performance test results are shown in Table 1 and Table 2

[0123] Table 1

[0124]

[0125]

[0126]

[0127]

[0128]

[0129]

[0130] Table 2

[0131]

[0132]

[0133]

[0134] Combining Example 1 and Comparative Examples 1-3 and Table 1-2, it can be seen that compared with Comparative Examples 1-3, Example 1 not only has higher tensile strength and flexural strength, but also has a higher sterilization rate, and after 4 cycles of corrosion in artificial seawater, it still has excellent tensile strength and flexural strength. This shows that the raw material ratio and preparation method of Example 1 can simultaneously improve the water resistance, corrosion resistance and microbial resistance of the FRP composite material.

[0135] Combining Examples 1-10 and Table 1-2, it can be seen that the tensile strength and bending strength of Examples 8 and 10 are relatively low, and Example 9 shows slight corrosion marks after 4 cycles of corrosion in artificial seawater. This shows that the raw material ratio of Examples 1-7 is helpful to further improve the physical properties, water resistance and corrosion resistance of the FRP composite material.

[0136] Combining Examples 1, 11-20 and Tables 1-2, it can be seen that Examples 15, 18 and 19 have higher tensile strength and flexural strength, which indicates that the use of basalt fiber and glass fiber in a weight ratio of 1: (0.4-0.7) can improve the physical properties of the FRP composite material.

[0137] It can be seen from Examples 1, 21-22 and Tables 1-2 that Example 21 has a higher sterilization rate, which indicates that the use of (2-methyl-5-nitrophenyl)guanidine nitrate can help further improve the microbial resistance of the FRP composite material.

[0138] It can be seen from Examples 1, 23-25 ​​and Tables 1-2 that after four cycles of corrosion testing at an artificial seawater temperature of 2±1°C, Example 25 showed obvious signs of corrosion, and after four cycles of corrosion testing at an artificial seawater temperature of 35±1°C, slight signs of corrosion appeared. This shows that the use of polysiloxanes containing perfluorobutane chains, perfluorohexane chains or perfluorooctane chains in the side chain structure can help further improve the water resistance, corrosion resistance and microbial resistance of FRP composite materials in low-temperature water environments.

[0139] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A FRP composite material, characterized in that: The invention comprises the following components in parts by weight: 30-50 parts of vinyl ester resin, 40-60 parts of epoxy resin, 2-5 parts of fluorine-containing silicone, 2-4 parts of triphenyltin chloride, 1-3 parts of organic guanidine compound, 1-3 parts of coupling agent, 1-3 parts of antioxidant, and 15-30 parts of reinforcing fiber; The fluorinated organosilicon is a polysiloxane containing a perfluoroalkyl chain in the side chain structure; The perfluoroalkyl chain is any one of a perfluorobutyl chain, a perfluorohexyl chain or a perfluorooctyl chain; The organic guanidine compound is at least one of 1,3-diaminoguanidine hydrochloride, (2-methyl-5-nitrophenyl)guanidine nitrate, and diethylguanidine sulfate.

2. The FRP composite material according to claim 1, characterized in that: The organic guanidine compound is (2-methyl-5-nitrophenyl)guanidine nitrate.

3. The FRP composite material according to claim 1, characterized in that: The epoxy resin is a mixture of bisphenol A epoxy resin and flexible aliphatic epoxy resin in a weight ratio of 1:(0.6-1.5).

4. The FRP composite material according to claim 1, characterized in that: The reinforcing fiber includes at least one of glass fiber, carbon fiber or basalt fiber.

5. The FRP composite material according to claim 4, characterized in that: The reinforcing fiber is a mixture of basalt fiber and glass fiber in a weight ratio of 1: (0.4-0.7).

6. A method for preparing the FRP composite material according to any one of claims 1 to 5, characterized in that: The steps include: Premixing: Evenly mix the vinyl ester resin, epoxy resin, fluorinated silicone, triphenyltin chloride and organic guanidine compound to obtain a mixture A; evenly mix the coupling agent, antioxidant and reinforcing fiber to obtain a mixture B; Molding: Mix mixture A and mixture B evenly to obtain mixture C, pour mixture C into a mold, discharge bubbles in mixture C, place the mold at 82-88°C, heat for 2.2-2.6h, then place it at 135-142°C, heat for 3-4h, end heating, cool and demold to obtain an FRP composite material.

7. Use of the FRP composite material according to any one of claims 1 to 6 in aquaculture ponds, characterized in that: The FRP composite material is used to prepare any structure or component in a breeding pond.