In-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material and preparation method thereof

By using phytic acid modified black phosphorus two-dimensional nanosheets and melamine to form an in-situ three-dimensional assembly structure in silicone rubber, the problem of insufficient flame retardant and electromagnetic shielding performance in the field of new energy vehicles is solved, and high mechanical strength is achieved and excellent electromagnetic shielding effect.

CN118496670BActive Publication Date: 2024-11-12WUHAN GEMEI INTELLIGENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410656331.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-11-12
Estimated Expiration
2044-05-24

AI Technical Summary

Technical Problem

At present, there is a gap between the flame retardant performance and electromagnetic shielding performance and application requirements in the field of new energy vehicles, and the flammable nature limits its application.

Method used

Phytic acid modified black phosphorus two-dimensional nanosheets and melamine form an in-situ three-dimensional assembly structure in silicon rubber, and generates active free radicals and inert gas release through high temperature decomposition, forms dense carbon layers and multi-layer conductive networks to improve flame retardant and Electromagnetic shielding performance.

Benefits of technology

The flame retardant, electromagnetic shielding and mechanical properties of silicone rubber composite materials have been significantly improved, and the requirements of new energy vehicles for polymer materials are met, achieving high mechanical strength, high flame retardant performance and excellent electromagnetic shielding effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118496670B_ABST
    Figure CN118496670B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a flame-retardant, reinforced and electromagnetic shielding silicone rubber composite material assembled in situ three-dimensionally, comprising the following steps: Step 1: Preparation of phytic acid-modified black phosphorus two-dimensional nanosheets; Step 2: Preparation of stripped phytic acid-modified black phosphorus two-dimensional nanosheets; Step 3: Preparation of silicone rubber composite sheet materials; Step 4: Preparation of flame-retardant, reinforced and electromagnetic shielding silicone rubber composite material assembled in situ three-dimensionally. In the present invention, the technology of phytic acid stripping black phosphorus is not only efficient, but also after introducing phytic acid on the surface of black phosphorus, it gives it the ability to react with other chemicals and form a three-dimensional network. At the same time, the silicone rubber composite material has both high mechanical strength, high flame retardancy and electromagnetic shielding properties, which is very consistent with the requirements of new energy vehicles for polymer materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer additives, and in particular relates to an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material and a preparation method thereof. Background Art

[0002] In recent years, the intensification of the global greenhouse effect and the increasing depletion of fossil energy have restricted the development of traditional fuel vehicles, and new energy vehicles have come into being.

[0003] Due to the active chemical properties of the battery itself, new energy vehicles cannot release the heat of the battery, causing the battery temperature and pressure to rise rapidly, and finally thermal runaway. At the same time, the high-temperature spontaneous combustion of new energy vehicles may also be caused by the charging and discharging process and environmental factors. The spontaneous combustion problem of new energy vehicles has become an important bottleneck restricting the development of new energy vehicles.

[0004] In addition, since batteries are prone to release magnetic fields, especially low-frequency magnetic fields, during charging and discharging and during the conversion of AC and DC, studies have shown that long-term exposure to low-frequency magnetic fields can cause certain harm to the human body. Therefore, polymer materials are widely used in new energy vehicles, and how to improve the flame retardant and electromagnetic shielding properties of polymer materials has become an important issue in the development of new energy vehicles.

[0005] Silicone rubber refers to a rubber whose main chain is composed of alternating silicon and oxygen atoms, and the silicon atom is usually connected to two organic groups. It has excellent heat resistance, cold resistance, corrosion resistance and plasticity, and has a wide range of applications in the field of new energy vehicles. However, there is still a certain gap between the flame retardant properties and electromagnetic shielding properties of silicone rubber at this stage and the application requirements of new energy vehicles. Therefore, how to improve the flame retardancy and electromagnetic shielding of silicone rubber composite materials is the key to expanding the use of silicone rubber in the field of new energy vehicles.

[0006] The flammable nature of silicone rubber limits its application in the field of new energy vehicles, so it is necessary to modify silicone rubber to make it flame retardant. Commonly used flame retardant additives include halogen flame retardants, inorganic metal compound flame retardants, phosphorus nitrogen flame retardants, and carbon materials.

[0007] Halogen flame retardants contain a large amount of halogens and produce a large amount of toxic gases, so their use is greatly restricted. The flame retardant efficiency of inorganic metal compounds is low, and a large amount of flame retardants need to be added to achieve a good flame retardant effect. Carbon materials mainly play a carbon-forming role and are generally used in conjunction with other flame retardants. Phosphorus-nitrogen flame retardants have excellent synergistic effects, with condensed phase flame retardant and gas phase flame retardant effects. Summary of the invention

[0008] The technical problem solved by the present invention is that the flame retardant performance and electromagnetic shielding performance of silicone rubber at the current stage still have a gap with the requirements of new applications.

[0009] In view of the technical problems existing in the prior art, the present invention designs an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material.

[0010] In order to solve the above-mentioned technical problems, the present invention adopts the following solutions:

[0011] A method for preparing an in-situ three-dimensionally assembled flame-retardant, reinforced, and electromagnetic shielding silicone rubber composite material, characterized in that it comprises the following steps:

[0012] Step 1: Preparation of phytic acid modified black phosphorus two-dimensional nanosheets;

[0013] Step 2: Preparation of exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets;

[0014] Step 3: Preparation of silicone rubber composite sheet material;

[0015] Step 4: Preparation of in-situ three-dimensionally assembled flame-retardant, reinforced, and electromagnetic shielding silicone rubber composites.

[0016] Furthermore, the specific steps of preparing the phytic acid-modified black phosphorus two-dimensional nanosheets in step 1 are:

[0017] Step 1: Grind black phosphorus in a mortar, mix the ground black phosphorus with phytic acid in a polytetrafluoroethylene autoclave, introduce nitrogen, add a solvent, seal and perform heat treatment to obtain phytic acid-modified black phosphorus two-dimensional nanosheets;

[0018] The specific steps of preparing the phytic acid-modified black phosphorus two-dimensional nanosheets peeled off in step 2 are:

[0019] Step 2: ultrasonically exfoliating the phytic acid modified black phosphorus two-dimensional nanosheets obtained in step 1, centrifuging them, and vacuum drying the supernatant of the phytic acid modified black phosphorus nanosheets after centrifugation to obtain exfoliated phytic acid modified black phosphorus two-dimensional nanosheets;

[0020] The specific steps of preparing the silicone rubber composite sheet material in step 3 are:

[0021] Step 3: heating, shearing and plasticizing the peeled phytic acid-modified black phosphorus two-dimensional nanosheets, melamine and silicone rubber using a double-roll mill to obtain a silicone rubber composite sheet material;

[0022] The specific steps of preparing the in-situ three-dimensional assembly of the flame-retardant, reinforced, and electromagnetic shielding silicone rubber composite material in step 4 are as follows:

[0023] Step 4: The silicone rubber composite sheet material prepared in step 3 is subjected to two-stage curing in a flat vulcanizer to obtain an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material.

[0024] Furthermore, in step 1, the mass ratio of black phosphorus to phytic acid is 1.5:1-1:1.5;

[0025] The solvent is one of dimethyl sulfoxide, N,N-dimethylformamide, ethanol, methanol, acetone, and deionized water;

[0026] The dosage ratio of the phytic acid to the solvent is 40mg-50g:20ml;

[0027] The ventilation time of the nitrogen is 15min-25min;

[0028] The temperature of the heat treatment is 180° C.-220° C., and the reaction time is 20 h-30 h.

[0029] Furthermore, in step 2, in the ultrasonic peeling, the ultrasonic peeling power is 300w-400w, and the time is 60min-120min;

[0030] In the centrifuge, the centrifugal speed is 1200rpm-1800rpm, and the time is 15min-30min.

[0031] Furthermore, in step 3, the silicone rubber is methyl vinyl silicone rubber, and the molar content of vinyl groups is 0.1%-0.2%;

[0032] The ratio of the peeled phytic acid modified black phosphorus two-dimensional nanosheets: melamine: silicone rubber is 3-6phr: 3-6phr: 100phr.

[0033] Furthermore, in step 3, the roller distance of the double-roll mill is 0.3 min-0.4 min, the temperature is 30° C.-40° C., and the number of shearing and plasticizing times is 4-6 times.

[0034] Furthermore, in the two-stage curing in the flat vulcanizing agent described in step 4, the first stage curing temperature is 160° C.-180° C.; the pressure is normal pressure, and the time is 8 min-12 min.

[0035] Furthermore, in the two-stage curing in the flat vulcanizing agent described in step 4, the second stage curing temperature is 160° C.-180° C.; the pressure is 12 MPa-17 MPa, and the time is 4 min-6 min.

[0036] The invention also discloses an in-situ three-dimensionally assembled flame-retardant, reinforced and electromagnetic shielding silicone rubber composite material.

[0037] The invention also discloses an application of an in-situ three-dimensionally assembled flame-retardant, reinforced and electromagnetic shielding silicone rubber composite material in the field of new energy vehicles.

[0038] In the present invention, in order to further optimize the performance of the composite material, in step 1, the mass ratio of black phosphorus to phytic acid is preferably 1:1; the solvent is preferably dimethyl sulfoxide, and the usage ratio of phytic acid to solvent is preferably 40 mg:20 ml; the nitrogen ventilation time is preferably 20 min; the reaction temperature is preferably 200°C, and the reaction time is preferably 24 h.

[0039] In step 2, the ultrasonic power is preferably 350-370w, the time is preferably 80-100min; the centrifugal speed is preferably: 1500rpm; the time is preferably: 20min.

[0040] In step 3, the silicone rubber preferably has a vinyl group content of 0.17% by molar. The relative molecular mass of the silicone rubber is preferably 6.9×10 5 .

[0041] The ratio of the exfoliated phytic acid modified black phosphorus two-dimensional nanosheets: melamine: silicone rubber is preferably 4-5phr: 4-5phr: 100phr.

[0042] The roll gap of the two-roll mill is preferably 0.35 mm, the temperature is 35° C., and the number of times is 5.

[0043] In step 4, the first stage curing temperature is preferably 170-175°C, the pressure is normal pressure, and the curing time is 10 minutes;

[0044] The second stage curing temperature is preferably 170-175°C, the pressure is 15 MPa, and the curing time is 5 minutes.

[0045] In the present invention, black phosphorus nanosheets are successfully peeled off by phytic acid, and the schematic diagram of the peeling is shown in the attached figure. Figure 1 shown.

[0046] In the present invention, the reaction process of phytic acid and melamine is as follows: Figure 2 shown.

[0047] In the present invention, the strengthening, flame retardant and electromagnetic shielding mechanisms of the silicone rubber composite material are:

[0048] Firstly, in terms of flame retardancy, phosphorus element decomposes at high temperature to produce active free radicals to eliminate unstable free radicals, and nitrogen element releases inert gas to dilute combustible gas.

[0049] At the same time, the in-situ generated three-dimensional network structure can increase the melt strength of the matrix material and reduce the droplet phenomenon during combustion. The active sites of the black phosphorus sheet itself and the phosphorus element catalytic composite material form a dense carbon layer, isolating the contact between oxygen and flame, which quickly stops the flame combustion and achieves the purpose of flame retardancy.

[0050] Second, the black phosphorus sheets are oriented in a three-dimensional spatial network in silicone rubber to form a multi-layer conductive path. Due to the defects of black phosphorus itself, the electron cloud at the defect site will be irregularly distributed and aggregated, resulting in polarization loss and consumption of electromagnetic wave energy. The multi-layer spatial conductive network will increase the propagation path of the electromagnetic wave, causing the electromagnetic wave to be reflected and reabsorbed multiple times.

[0051] Third, trifunctional melamine and hexafunctional phytic acid-loaded black phosphorus nanosheets self-assemble in situ in the silicone rubber matrix to form a three-dimensional network structure, replacing the vulcanizing agent, causing the silicone rubber to cross-link and cure, and increasing the mechanical strength of the silicone rubber composite material.

[0052] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising" and similar meanings, and closed-ended "consisting of..." and similar meanings.

[0053] The present invention provides an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material and a preparation method thereof, which have the following beneficial effects:

[0054] (1) The phytic acid stripping black phosphorus technology in the silicone rubber composite material of the present invention is not only highly efficient, but also introduces phytic acid on the surface of black phosphorus, giving it the ability to react with other chemicals and form a three-dimensional network.

[0055] (2) The silicone rubber composite material of the present invention has an extremely excellent flame retardant effect. The phosphorus element decomposes at high temperature to produce active free radicals to remove unstable free radicals, and the nitrogen element releases inert gas to dilute the combustible gas. At the same time, the three-dimensional network structure generated in situ can increase the melt strength of the matrix material and reduce the droplet phenomenon during combustion. The active sites of the black phosphorus layer itself catalyze the composite material with the phosphorus element to form a dense carbon layer, isolating the contact between oxygen and flame, and quickly preventing the flame from burning, thereby achieving the purpose of flame retardancy.

[0056] (3) The silicone rubber composite material of the present invention has an extremely excellent electromagnetic shielding effect. The black phosphorus sheets are oriented in a three-dimensional network in the silicone rubber to form a multi-layer conductive path. Due to the defects of black phosphorus itself, the electron cloud at the defect is irregularly distributed and aggregated, resulting in polarization loss and consumption of electromagnetic wave energy.

[0057] Multi-layer spatial conductive networks will increase the propagation path of electromagnetic waves, causing electromagnetic waves to be reflected and reabsorbed multiple times.

[0058] (4) The silicone rubber composite material of the present invention has extremely excellent mechanical properties. The black phosphorus nanosheets loaded with trifunctional melamine and hexafunctional phytic acid are self-assembled in situ in the silicone rubber matrix to form a three-dimensional network structure, replacing the vulcanizing agent, causing the silicone rubber to cross-link and cure, thereby increasing the mechanical strength of the silicone rubber composite material.

[0059] (5) The silicone rubber composite material of the present invention has high mechanical strength, high flame retardancy, and electromagnetic shielding properties, which is in line with the requirements of new energy vehicles for polymer materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 : Schematic diagram of phytic acid stripping of a single layer of black phosphorus in the present invention;

[0061] Figure 2 : is a schematic diagram of the reaction of phytic acid and melamine in the present invention;

[0062] Figure 3 : Schematic diagram of the structural model of the in-situ three-dimensional assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material prepared by the present invention. DETAILED DESCRIPTION

[0063] The present invention will be further described below in conjunction with specific embodiments and accompanying drawings:

[0064] Example 1

[0065] Step 1: Preparation of phytic acid modified black phosphorus two-dimensional nanosheets;

[0066] After grinding the black phosphorus crystals in a mortar, 40 mg of the treated black phosphorus flakes, 40 mg of phytic acid and 20 ml of dimethyl sulfoxide were mixed in a 50 ml polytetrafluoroethylene autoclave, and nitrogen was introduced for 20 min to remove the air in the system. The system was then sealed and subjected to solvothermal treatment at 200 °C for 24 h to obtain phytic acid-modified black phosphorus two-dimensional nanosheets.

[0067] Step 2: Preparation of exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets;

[0068] The heat-treated phytic acid-modified black phosphorus two-dimensional nanosheets were subjected to 360W ultrasonic exfoliation for 100 minutes, and then centrifuged. The mixture was centrifuged at 1500rpm for 20 minutes, and the supernatant of the centrifuged phytic acid-modified black phosphorus nanosheets was collected and vacuum dried to obtain exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets.

[0069] Step 3: Preparation of silicone rubber composite sheet material;

[0070] The peeled phytic acid modified black phosphorus two-dimensional nanosheets, the ratio of melamine to silicone rubber is 4phr:4phr:100phr. The prepared silicone rubber composite material is sheared and plasticized 5 times with a 35°C double-roll mill with a roller gap of 0.35mm to obtain a silicone rubber composite sheet. The silicone rubber is methyl vinyl silicone rubber, and the molar content of vinyl groups is 0.7%.

[0071] Step 4: Preparation of in-situ three-dimensional assembly of flame-retardant, reinforced and electromagnetic shielding silicone rubber composites:

[0072] The prepared silicone rubber composite sheet material is cured in a standard mold at a first-stage curing temperature of 170°C, a normal pressure, and a curing time of 10 min; the second-stage curing temperature is 170°C, a pressure of 15 MPa, and a curing time of 5 min to obtain an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material.

[0073] like Figure 3 This is a schematic diagram of the structural model of the in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material prepared by the present invention.

[0074] Example 2

[0075] Step 1: Preparation of phytic acid modified black phosphorus two-dimensional nanosheets;

[0076] After grinding the black phosphorus crystals in a mortar, 40 mg of the treated black phosphorus flakes, 40 mg of phytic acid and 20 ml of dimethyl sulfoxide were mixed in a 50 ml polytetrafluoroethylene autoclave, and nitrogen was introduced for 20 min to remove the air in the system. The system was then sealed and solvothermal treated at 190 °C for 24 h to obtain phytic acid-modified black phosphorus two-dimensional nanosheets.

[0077] Step 2: Preparation of exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets;

[0078] The heat-treated phytic acid-modified black phosphorus two-dimensional nanosheets were subjected to 360W ultrasonic exfoliation for 60 minutes, and then centrifuged. The mixture was centrifuged at 1800rpm for 15 minutes, and the supernatant of the centrifuged phytic acid-modified black phosphorus nanosheets was collected and vacuum dried to obtain exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets.

[0079] Step 3: Preparation of silicone rubber composite sheet material;

[0080] The peeled phytic acid modified black phosphorus two-dimensional nanosheets, the ratio of melamine to silicone rubber is 4.5phr:4.5phr:100phr. The prepared silicone rubber composite material is sheared and plasticized 4 times using a 40°C double-roll open mill with a roller gap of 0.35mm to obtain a silicone rubber composite sheet. The silicone rubber is methyl vinyl silicone rubber, and the molar content of vinyl groups is 0.7%.

[0081] Step 4: Preparation of in-situ three-dimensional assembly of flame-retardant, reinforced and electromagnetic shielding silicone rubber composites:

[0082] The prepared silicone rubber composite sheet material is cured in a standard mold at a first-stage curing temperature of 175°C, a normal pressure, and a curing time of 8 minutes; the second-stage curing temperature is 175°C, a pressure of 15 MPa, and a curing time of 4 minutes to obtain an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material.

[0083] Example 3

[0084] Step 1: Preparation of phytic acid modified black phosphorus two-dimensional nanosheets;

[0085] After grinding the black phosphorus crystals in a mortar, 40 mg of the treated black phosphorus flakes, 40 mg of phytic acid and 20 ml of dimethyl sulfoxide were mixed in a 50 ml polytetrafluoroethylene autoclave, and nitrogen was introduced for 20 min to remove the air in the system. The system was then sealed and solvothermal treated at 210 °C for 28 h to obtain phytic acid-modified black phosphorus two-dimensional nanosheets.

[0086] Step 2: Preparation of exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets;

[0087] The heat-treated phytic acid-modified black phosphorus two-dimensional nanosheets were subjected to 360W ultrasonic exfoliation for 100 minutes, and then centrifuged. The mixture was centrifuged at 1500rpm for 20 minutes, and the supernatant of the centrifuged phytic acid-modified black phosphorus nanosheets was collected and vacuum dried to obtain exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets.

[0088] Step 3: Preparation of silicone rubber composite sheet material;

[0089] The peeled phytic acid modified black phosphorus two-dimensional nanosheets, the ratio of melamine to silicone rubber is 5phr:5phr:100phr. The prepared silicone rubber composite material is sheared and plasticized 5 times with a 35°C double-roll open mill with a roller gap of 0.35mm to obtain a silicone rubber composite sheet. The silicone rubber is methyl vinyl silicone rubber, and the molar content of vinyl groups is 0.7%.

[0090] Step 4: Preparation of in-situ three-dimensional assembly of flame-retardant, reinforced and electromagnetic shielding silicone rubber composites:

[0091] The prepared silicone rubber composite sheet material is cured in a standard mold at a first-stage curing temperature of 170°C, a normal pressure, and a curing time of 10 min; the second-stage curing temperature is 170°C, a pressure of 15 MPa, and a curing time of 5 min to obtain an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material.

[0092] Example 4

[0093] Step 1: Preparation of phytic acid modified black phosphorus two-dimensional nanosheets;

[0094] After grinding the black phosphorus crystals in a mortar, 40 mg of the treated black phosphorus flakes, 60 mg of phytic acid and 20 ml of N,N-dimethylformamide were mixed in a 50 ml polytetrafluoroethylene autoclave, and nitrogen was introduced for 15 min to remove the air in the system. The system was then sealed and solvothermal treated at 180 °C for 30 h to obtain phytic acid-modified black phosphorus two-dimensional nanosheets.

[0095] Step 2: Preparation of exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets;

[0096] The heat-treated phytic acid-modified black phosphorus two-dimensional nanosheets were subjected to 300W ultrasonic exfoliation for 120 minutes, and then centrifuged. The mixture was centrifuged at 1200rpm for 30 minutes, and the supernatant of the centrifuged phytic acid-modified black phosphorus nanosheets was collected and vacuum dried to obtain exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets.

[0097] Step 3: Preparation of silicone rubber composite sheet material;

[0098] The peeled phytic acid modified black phosphorus two-dimensional nanosheets, the ratio of melamine to silicone rubber is 3phr:3phr:100phr. The prepared silicone rubber composite material is sheared and plasticized 6 times using a 30°C double-roll open mill with a roller gap of 0.3mm to obtain a silicone rubber composite sheet. The silicone rubber is methyl vinyl silicone rubber, and the molar content of vinyl groups is 0.7%.

[0099] Step 4: Preparation of in-situ three-dimensional assembly of flame-retardant, reinforced and electromagnetic shielding silicone rubber composites:

[0100] The prepared silicone rubber composite sheet material is cured in a standard mold at a first-stage curing temperature of 160°C, a normal pressure, and a curing time of 12 min; the second-stage curing temperature is 160°C, a pressure of 12 MPa, and a curing time of 6 min to obtain an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material.

[0101] Example 5

[0102] Step 1: Preparation of phytic acid modified black phosphorus two-dimensional nanosheets;

[0103] After grinding the black phosphorus crystals in a mortar, 60 mg of the treated black phosphorus flakes, 40 mg of phytic acid and 20 ml of acetone were mixed in a 50 ml polytetrafluoroethylene autoclave, and nitrogen was introduced for 25 min to remove the air in the system. The system was then sealed and subjected to solvothermal treatment at 220 °C for 20 h to obtain phytic acid-modified black phosphorus two-dimensional nanosheets.

[0104] Step 2: Preparation of exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets;

[0105] The heat-treated phytic acid-modified black phosphorus two-dimensional nanosheets were subjected to 400W ultrasonic exfoliation for 60 minutes, and then centrifuged. The mixture was centrifuged at 1800rpm for 15 minutes, and the supernatant of the centrifuged phytic acid-modified black phosphorus nanosheets was collected and vacuum dried to obtain exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets.

[0106] Step 3: Preparation of silicone rubber composite sheet material;

[0107] The peeled phytic acid modified black phosphorus two-dimensional nanosheets, the ratio of melamine to silicone rubber is 6phr:6phr:100phr. The prepared silicone rubber composite material is sheared and plasticized 6 times using a 40°C double-roll open mill with a roller gap of 0.4mm to obtain a silicone rubber composite sheet. The silicone rubber is methyl vinyl silicone rubber, and the molar content of vinyl groups is 0.7%.

[0108] Step 4: Preparation of in-situ three-dimensional assembly of flame-retardant, reinforced and electromagnetic shielding silicone rubber composites:

[0109] The prepared silicone rubber composite sheet material is cured in a standard mold at a first-stage curing temperature of 180°C, a normal pressure, and a curing time of 8 minutes; the second-stage curing temperature is 180°C, a pressure of 17 MPa, and a curing time of 4 minutes to obtain an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material.

[0110] Comparative Example 1

[0111] The difference from Example 1 is the preparation formula of the silicone rubber composite sheet material. The preparation formula of the silicone rubber composite sheet material in Comparative Example 1 is calculated by mass fraction as follows: 90 wt % of addition silicone rubber and 10 wt % of flame retardant aluminum hydroxide.

[0112] Comparative Example 2

[0113] The difference from Example 1 is the preparation formula of the silicone rubber composite sheet material. The preparation formula of the silicone rubber composite sheet material in Comparative Example 2 is calculated by mass fraction as follows: 90 wt % of addition silicone rubber and 10 wt % of flame retardant ammonium polyphosphate.

[0114] About performance testing and description:

[0115] With reference to the national standards "GB / T 1040 Determination of tensile properties of plastics", "GB 2409-84 Vertical combustion method", and "ISO4589 Limiting oxygen index (LOI)", the hardness is measured by LX-A Shaw rubber hardness tester.

[0116] The test standard is GB / T2411-2008, and the volume resistivity and surface resistance are tested according to GB / T2439-2001.

[0117] The dielectric properties and electromagnetic shielding performance tests are required to be carried out at 25°C and 4-12GHz X-band frequency.

[0118] Table 1. Results of silicone rubber composite material performance test

[0119]

[0120]

[0121] Table 2. Results of silicone rubber composite material performance test

[0122]

[0123] Analysis of the test results:

[0124] It can be seen from the test results in Table 1 and Table 2 that, firstly, the silicone rubber composite material with the in-situ three-dimensional network structure provided by the present invention has excellent tensile strength, elongation at break and hardness, which can reach up to 3.70 MPa, 284% and 76.5A.

[0125] In addition, the amount of the silicone rubber composite material prepared by the present invention is much lower than that of conventional flame-retardant silicone rubber on the market. While meeting the flame-retardant requirements, the mechanical properties are better than those of conventional flame-retardant silicone rubber.

[0126] The in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber obtained by this preparation method has flame-retardant properties and at the same time enables the silicone rubber material to have high strength and excellent electromagnetic shielding properties.

[0127] In the present invention, the technology of phytic acid stripping black phosphorus is not only highly efficient, but also gives it the ability to react with other chemicals and form a three-dimensional network after the phytic acid is introduced on the surface of black phosphorus. At the same time, the silicone rubber composite material has high mechanical strength, high flame retardancy and electromagnetic shielding properties, which is very consistent with the requirements of new energy vehicles for polymer materials.

[0128] The present invention is described exemplarily above in conjunction with the embodiments and drawings. It is obvious that the implementation of the present invention is not limited to the above-mentioned methods. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A method for preparing an in-situ three-dimensionally assembled flame-retardant, reinforced, and electromagnetic shielding silicone rubber composite material, characterized in that: The steps include: Step 1: Preparation of phytic acid modified black phosphorus two-dimensional nanosheets; Step 2: Preparation of exfoliated phytic acid-modified black phosphorus two-dimensional nanosheets; Step 3: Preparation of silicone rubber composite sheet material; Step 4: Preparation of in-situ three-dimensional assembly of flame-retardant, reinforced, and electromagnetic shielding silicone rubber composites; The specific steps of preparing the phytic acid-modified black phosphorus two-dimensional nanosheets in step 1 are: Step 1: Grind black phosphorus in a mortar, mix the ground black phosphorus with phytic acid in a polytetrafluoroethylene autoclave, introduce nitrogen, add a solvent, seal and perform heat treatment to obtain phytic acid-modified black phosphorus two-dimensional nanosheets; The specific steps of preparing the phytic acid-modified black phosphorus two-dimensional nanosheets peeled off in step 2 are: Step 2: ultrasonically exfoliating the phytic acid modified black phosphorus two-dimensional nanosheets obtained in step 1, centrifuging them, and vacuum drying the supernatant of the phytic acid modified black phosphorus nanosheets after centrifugation to obtain exfoliated phytic acid modified black phosphorus two-dimensional nanosheets; The specific steps of preparing the silicone rubber composite sheet material in step 3 are: Step 3: heating, shearing and plasticizing the peeled phytic acid-modified black phosphorus two-dimensional nanosheets, melamine and silicone rubber using a double-roll mill to obtain a silicone rubber composite sheet material; The specific steps of preparing the in-situ three-dimensional assembly of the flame-retardant, reinforced, and electromagnetic shielding silicone rubber composite material in step 4 are as follows: Step 4: The silicone rubber composite sheet material prepared in step 3 is subjected to two-stage curing in a flat vulcanizer to obtain an in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material.

2. The method for preparing the in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material according to claim 1, characterized in that: In step 1, the mass ratio of black phosphorus to phytic acid is 1.5:1-1:1.5; The solvent is one of dimethyl sulfoxide, N,N-dimethylformamide, ethanol, methanol, acetone, and deionized water; The dosage ratio of the phytic acid to the solvent is 40mg-50g:20ml; The ventilation time of the nitrogen is 15min-25min; The temperature of the heat treatment is 180° C.-220° C., and the reaction time is 20 h-30 h.

3. The method for preparing the in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material according to claim 1, characterized in that: In step 2, in the ultrasonic peeling, the ultrasonic peeling power is 300w-400w, and the time is 60min-120min; In the centrifuge, the centrifugal speed is 1200rpm-1800rpm, and the time is 15min-30min.

4. The method for preparing the in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material according to claim 1, characterized in that: In step 3, the silicone rubber is methyl vinyl silicone rubber, and the molar content of vinyl groups is 0.1%-0.2%; The ratio of the peeled phytic acid modified black phosphorus two-dimensional nanosheets: melamine: silicone rubber is 3-6phr: 3-6phr: 100phr.

5. The method for preparing the in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material according to claim 1, characterized in that: In step 3, the roller distance of the double-roll mill is 0.3 min-0.4 min, the temperature is 30° C.-40° C., and the number of shearing and plasticizing times is 4-6 times.

6. The method for preparing the in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material according to claim 5, characterized in that: In step 4, the two-stage curing is carried out in a flat vulcanizer, wherein the first stage curing temperature is 160° C.-180° C.; the pressure is normal pressure, and the time is 8 min-12 min.

7. The method for preparing the in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material according to claim 5, characterized in that: In step 4, the second stage curing is carried out in a flat vulcanizing press, wherein the second stage curing temperature is 160° C.-180° C.; the pressure is 12 MPa-17 MPa, and the time is 4 min-6 min.

8. An in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material, characterized in that: The composite material is prepared according to the preparation method according to any one of claims 1 to 7.

9. An application of the in-situ three-dimensionally assembled flame-retardant, reinforced, electromagnetic shielding silicone rubber composite material as claimed in claim 8 in the field of new energy vehicles.