A flame retardant high insulation epoxy composite material and preparation method thereof
By using flame retardant toughening agents and accelerated dicyandiamide curing agents in epoxy composite materials, the problem of poor flame retardancy and insulation of epoxy composite materials in the existing technology is solved, and the insulation performance and insulation properties of the material are improved. Flame retardant, suitable for high humidity environments and has good wear resistance and water resistance.
Patent Information
- Application Number
- CN202410932820.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Existing epoxy composite materials have poor flame retardancy and insulation and cannot meet the needs of communication technology for excellent thermal properties, low relative dielectric constant, low dissipation factor and flame retardancy.
Use bisphenol A type epoxy resin, fillers, leveling agents, accelerators, defoaming agents and flame retardant toughening agents to prepare component A in a specific proportion, and prepare component B with accelerated dicyandiamide curing agent. The flame-retardant high-insulation epoxy composite material is prepared by mixing, cooling, tableting, and grinding in a twin-screw extruder. The flame-retardant toughening agent reduces the dielectric constant through the medium fluorine functional group and Si-C bond, and decomposes to produce flame-retardant gas. and phosphoric acid derivatives to enhance flame retardancy.
The insulation performance, impact strength, tensile strength, bending strength and flame retardant properties of the flame-retardant high-insulation epoxy composite material are improved, achieving a balance of fire safety and smoke suppression, and at the same time, it has high solid content, safety and environmental protection, and film-forming properties. It has good durability, wear resistance and water resistance, and is suitable for high humidity environments.
Smart Images

Figure CN118496738B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder coatings, and in particular relates to a flame-retardant high-insulation epoxy composite material and a preparation method thereof. Background Art
[0002] Powder coating is a solid powdered synthetic resin coating composed of solid resin, pigment, filler and additives. Powder coating is different from ordinary solvent-based coating and water-based coating in that its dispersion medium is not solvent and water, but air. It has the characteristics of no solvent pollution, 100% film formation and low energy consumption. Epoxy resin (EP) is widely used in various fields such as electronics, coatings and adhesives due to its excellent mechanical properties, good corrosion resistance and excellent adhesion. However, in view of the rapid development of communication technology, the demand for epoxy resin (EP) has emerged with supplementary properties, such as excellent thermal properties, low relative dielectric constant, low dissipation factor, flame retardancy, etc. Therefore, there is an urgent need for an epoxy composite material with good flame retardancy and insulation to solve the above problems. Summary of the invention
[0003] The object of the present invention is to provide a flame retardant high-insulation epoxy composite material and a preparation method thereof, so as to solve the technical problem of poor flame retardancy and poor insulation of epoxy composite materials in the prior art.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] The technical solution provided by the present invention is as follows:
[0006] In the first aspect, the present invention provides a flame retardant high-insulation epoxy composite material, which includes two components A and B. Component A contains, by weight: 70-90 parts of bisphenol A epoxy resin, 30-40 parts of filler, 2-3 parts of leveling agent, 2-3 parts of accelerator, 0.7-1.2 parts of defoaming agent, and 5-8 parts of flame retardant toughening agent; component B is 6.5-8.5 parts of accelerated dicyandiamide curing agent.
[0007] Preferably, the method for preparing the flame retardant toughening agent comprises the following steps:
[0008] S1: Add 12.9-26 g of p-aminotrifluorotoluene and 11-22 g of 2,5-dihydroxybenzaldehyde to 100-200 mL of ethanol, stir for 3-5 h, filter, wash the filter residue with ethanol 3-5 times, add the filter residue to 200-400 mL of ethanol, heat at 75-85 ° C for 30-50 min, then add 17.3-34.6 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide at 75-85 ° C, stir continuously for 20-28 h, filter while hot, wash the filter cake with ethanol 3-5 times, and finally vacuum dry at 55-65 ° C for 24-36 h to obtain an intermediate;
[0009] The structural formula of the intermediate is as follows:
[0010]
[0011] Among them, the intermediates were subjected to mass spectrometry analysis, HRMS (ESI) m / z: 483.08 (100.0%), 484.09 (27.4%), 485.09 (4.5%).
[0012] S2: Under a nitrogen atmosphere, 14.5-29 g of the intermediate and 4.1-8.2 g of triethylamine are added to 50-100 mL of N,N-dimethylformamide to obtain a mixed solution; then 2.8-5.6 g of phenyltrichlorosilane is dissolved in 40-80 mL of tetrahydrofuran and slowly added to the mixed solution through a dropping funnel, stirred at room temperature for 2-4 h, then stirred at 45-55 ° C for 1-3 h, filtered, and rotary evaporated at 85-95 ° C, and finally vacuum dried at 85-95 ° C for 20-28 h to obtain a flame retardant toughening agent.
[0013] The structural formula of the flame retardant toughening agent is as follows:
[0014]
[0015] Preferably, the filler is compounded from titanium dioxide, silicon powder and light calcium carbonate in a mass ratio of (10-12):(3-5):(3-4).
[0016] Preferably, the accelerator is dimethylimidazole.
[0017] Preferably, the defoaming agent is a polyoxyethylene polyoxypropanolamine ether defoaming agent.
[0018] Preferably, the curing agent is an accelerated dicyandiamide curing agent.
[0019] Preferably, the leveling agent is PV88 leveling agent.
[0020] In a second aspect, the present invention further provides a method for preparing a flame retardant high-insulation epoxy composite material, comprising the following steps:
[0021] Step (1) 70-90 parts of bisphenol A epoxy resin, 30-40 parts of filler, 2-3 parts of leveling agent, 2-3 parts of accelerator, 0.7-1.2 parts of defoamer and 5-8 parts of flame retardant toughening agent are added into a mixer for premixing, and then mixed and extruded by a twin-screw extruder, and after extrusion, cooled, tableted, crushed, ground and screened to obtain component A; component B is 6.5-8.5 parts of accelerated dicyandiamide curing agent;
[0022] Step (2) Evenly mix component A and component B to obtain a flame retardant high insulation epoxy composite material.
[0023] The heating temperature of the extruder is 90-110°C.
[0024] Preferably, the D50 particle size of the flame-retardant high-insulation epoxy composite material is 30-40 μm.
[0025] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0026] 1. The fluorine functional group in the flame retardant toughening agent prepared by the present invention can reduce the surface tension of the flame retardant high-insulation epoxy composite material, enhance hydrophobicity, and reduce the water content, thereby reducing the dielectric constant and dielectric loss; at the same time, the increase in free volume provided by the cavity inside the flame retardant toughening agent molecule reduces the density of polarized molecules, and the Si-C bond reduces the polarization rate of the matrix resin, synergistically reducing the dielectric constant and dielectric loss of the flame retardant high-insulation epoxy composite material, and synergistically cooperating with the insulating filler to improve the insulation performance of the flame retardant high-insulation epoxy composite material.
[0027] 2. The flame retardant and toughening agent in the present invention thermally decomposes in the gas phase to produce phosphorus-containing free radicals, including PO2˙ and PO˙, which capture combustion free radicals and reduce combustible hydrocarbons. At the same time, the flame retardant and toughening agent will also decompose to produce non-combustible gases, including NH3, N2 and HF, which play a flame retardant role in the gas phase; the flame retardant and toughening agent thermally decomposes in the condensed phase to produce phosphoric acid derivatives, which promote the development of the extended carbon layer. P and Si elements promote the formation of a continuous and dense hybrid carbon layer in the flame retardant high-insulation epoxy composite material during the combustion process, which effectively hinders the combustion in the condensed phase; the synergistic flame retardancy of P, N, and Si elements enhances the flame retardancy of the gas phase and the condensed phase, thereby achieving a balance between fire safety and smoke suppression for the flame retardant high-insulation epoxy composite material.
[0028] 3. The increase in the free volume of the flame retardant toughening agent and the increase in Si-O flexible bonds in the present invention improve the impact strength of the flame retardant high-insulation epoxy composite material. The flame retardant toughening agent is evenly distributed in the matrix resin through the covalent bonds and hydrogen bonds formed between the terminal hydroxyl groups and the epoxy resin, thereby enhancing the interfacial bonding force with the epoxy resin. At the same time, the increase in rigid groups improves the tensile strength and bending strength of the flame retardant high-insulation epoxy composite material. The combined effect of abundant rigid groups, Si-O flexible segments, increased free volume and good interfacial bonding cooperates with the composite filler to improve the strength and toughness of the flame retardant high-insulation epoxy composite material.
[0029] 4. The flame-retardant high-insulation epoxy composite material prepared by the present invention has a high solid content, is safe and environmentally friendly, has good film-forming properties, can form a film of 500 μm in one coat, can meet performance requirements with a single spray, has excellent wear resistance, high Shore hardness, and an average annual friction loss of only 0.012%. It also has excellent water resistance and can maintain performance under long-term high humidity or water immersion conditions. It has good adhesion and can be effectively attached to the outside of the equipment without peeling or falling off. It has excellent flame retardant properties and excellent insulation properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 The present invention is a flow chart of the preparation process of the flame-retardant high-insulation epoxy composite material. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] This embodiment discloses a method for preparing a flame retardant toughening agent, comprising the following steps:
[0035] S1: Add 19.5 g of p-aminotrifluorotoluene and 15.5 g of 2,5-dihydroxybenzaldehyde to 150 mL of ethanol, stir for 4 h, filter, wash the filter residue with ethanol 4 times, add the filter residue to 300 mL of ethanol, heat at 80 ° C for 40 min, then add 26 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide at 80 ° C, stir continuously for 24 h, filter while hot, wash the filter cake with ethanol 4 times, and finally vacuum dry at 60 ° C for 30 h to obtain an intermediate;
[0036] S2: Under a nitrogen atmosphere, 21.8 g of the intermediate and 6.2 g of triethylamine were added to 75 mL of N,N-dimethylformamide to obtain a mixed solution; then 4.2 g of phenyltrichlorosilane was dissolved in 60 mL of tetrahydrofuran and slowly added to the mixed solution through a dropping funnel, stirred at room temperature for 3 h, then stirred at 50 ° C for 2 h, filtered, and rotary evaporated at 90 ° C, and finally vacuum dried at 90 ° C for 24 h to obtain a flame retardant toughening agent.
[0037] Example 2
[0038] See also Figure 1 As shown, this embodiment discloses a method for preparing a flame retardant high insulation epoxy composite material, comprising the following steps:
[0039] Step (1) 80g of bisphenol A epoxy resin, 35g of filler, 2.5g of leveling agent, 2.5g of accelerator, 0.9g of defoamer and 7g of flame retardant toughening agent are added into a mixer for premixing, and then mixed and extruded at 100°C by a twin-screw extruder, and after extrusion, cooled, tableted, crushed, ground and screened to obtain component A; component B is 7.5g of accelerated dicyandiamide curing agent;
[0040] Step (2) Evenly mix component A and component B to obtain a flame retardant high insulation epoxy composite material.
[0041] Example 3
[0042] See also Figure 1 As shown, this embodiment discloses a method for preparing a flame retardant high insulation epoxy composite material, comprising the following steps:
[0043] Step (1) 70g of bisphenol A epoxy resin, 40g of filler, 2g of leveling agent, 3g of accelerator, 0.7g of defoamer and 8g of flame retardant toughening agent are added into a mixer for premixing, and then mixed and extruded at 90°C by a twin-screw extruder, and after extrusion, cooled, tableted, crushed, ground and screened to obtain component A; component B is 8.5g of accelerated dicyandiamide curing agent;
[0044] Step (2) Evenly mix component A and component B to obtain a flame retardant high insulation epoxy composite material.
[0045] Example 4
[0046] See also Figure 1 As shown, this embodiment discloses a method for preparing a flame retardant high insulation epoxy composite material, comprising the following steps:
[0047] Step (1) 90g of bisphenol A epoxy resin, 30g of filler, 3g of leveling agent, 2g of accelerator, 1.2g of defoamer and 5g of flame retardant toughening agent are added into a mixer for premixing, and then mixed and extruded at 90-110°C by a twin-screw extruder, and after extrusion, cooled, tableted, crushed, ground and screened to obtain component A; component B is 6.5-8.5g of accelerated dicyandiamide curing agent;
[0048] Step (2) Evenly mix component A and component B to obtain a flame retardant high insulation epoxy composite material.
[0049] Example 5
[0050] See also Figure 1 As shown, this embodiment discloses a method for preparing a flame retardant high insulation epoxy composite material, comprising the following steps:
[0051] Step (1) 75 g of bisphenol A epoxy resin, 48 g of filler, 2.2 g of leveling agent, 2.8 g of accelerator, 0.8 g of defoamer and 7 g of flame retardant toughening agent are added to a mixer for premixing, and then mixed and extruded at 95° C. using a twin-screw extruder, and after extrusion, cooled, tableted, crushed, ground and screened to obtain component A; component B is 8 g of an accelerated dicyandiamide curing agent;
[0052] Step (2) Evenly mix component A and component B to obtain a flame retardant high insulation epoxy composite material.
[0053] Example 6
[0054] See also Figure 1 As shown, this embodiment discloses a method for preparing a flame retardant high insulation epoxy composite material, comprising the following steps:
[0055] Step (1) 85 g of bisphenol A epoxy resin, 32 g of filler, 2.8 g of leveling agent, 2.2 g of accelerator, 1.1 g of defoamer and 6 g of flame retardant toughening agent are added into a mixer for premixing, and then mixed and extruded at 105° C. using a twin-screw extruder, and after extrusion, cooled, tableted, crushed, ground and screened to obtain component A; component B is 7 g of accelerated dicyandiamide curing agent;
[0056] Step (2) Evenly mix component A and component B to obtain a flame retardant high insulation epoxy composite material.
[0057] Comparative Example 1
[0058] Comparative Example 1 Compared with Example 2, in the process of preparing the flame-retardant high-insulation epoxy composite material, no flame retardant toughening agent was added in Comparative Example 1, and other conditions remained unchanged.
[0059] Comparative Example 2
[0060] Comparative Example 2 Compared with Example 2, in the process of preparing the flame-retardant high-insulation epoxy composite material, no filler was added in Comparative Example 2, and other conditions remained unchanged.
[0061] Experimental example
[0062] The flame-retardant high-insulation epoxy composite materials prepared in Examples 2-6 and Comparative Examples 1-2 were tested for their performance in groups A, B, C, D, E, F, and G. During the test, the AB components were stirred evenly (ethanol diluent should be added to the material for spraying with a vertical height greater than 10m, and 90-100mL / kg should be added in principle) and poured into the material tank, the air valve was opened, and the air pressure was adjusted (the tank air pressure indicated the number 0.3, and the outlet air pressure indicated the number 0.2). The nozzle was about 10-15cm away from the spraying point. When spraying, do not keep the nozzle at one point for too long. In principle, spray back and forth, and the dwell time at one point should not be greater than 2s. The test standards and test results are shown in Table 1:
[0063]
[0064] From the test results in Table 1, it can be seen that the flame-retardant high-insulation epoxy composite material prepared in Example 2 of the present invention has good insulation, mechanical properties and flame-retardant properties. From the comparison between Comparative Example 1 and Example 2, it can be seen that the addition of a flame-retardant toughening agent in the present invention can improve the insulation, mechanical properties and flame-retardant properties of the flame-retardant high-insulation epoxy composite material; from the comparison between Comparative Example 2 and Example 3, it can be seen that the addition of a filler in the present invention can improve the insulation, mechanical properties and flame-retardant properties of the flame-retardant high-insulation epoxy composite material.
[0065] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0066] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A flame retardant high insulation epoxy composite material, characterized in that: The flame-retardant high-insulation epoxy composite material comprises two components, A and B. Component A comprises 70-90 parts of bisphenol A epoxy resin, 30-40 parts of filler, 2-3 parts of leveling agent, 2-3 parts of accelerator, 0.7-1.2 parts of defoamer, and 5-8 parts of flame retardant toughening agent, and component B comprises 6.5-8.5 parts of accelerated dicyandiamide curing agent. The preparation method of the flame retardant toughening agent comprises the following steps: S1: Add 12.9-26 g of p-aminotrifluorotoluene and 11-22 g of 2,5-dihydroxybenzaldehyde to 100-200 mL of ethanol, stir for 3-5 h, filter, wash the filter residue with ethanol 3-5 times, add the filter residue to 200-400 mL of ethanol, heat at 75-85 ° C for 30-50 min, then add 17.3-34.6 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide at 75-85 ° C, stir continuously for 20-28 h, filter while hot, wash the filter residue with ethanol 3-5 times, and finally vacuum dry at 55-65 ° C for 24-36 h to obtain an intermediate; S2: Under a nitrogen atmosphere, 14.5-29 g of the intermediate and 4.1-8.2 g of triethylamine are added to 50-100 mL of N,N-dimethylformamide to obtain a mixed solution; then 2.8-5.6 g of phenyltrichlorosilane is dissolved in 40-80 mL of tetrahydrofuran, and slowly added to the mixed solution through a dropping funnel, stirred at room temperature for 2-4 h, then stirred at 45-55 ° C for 1-3 h, filtered, and rotary evaporated at 85-95 ° C, and finally vacuum dried at 85-95 ° C for 20-28 h to obtain a flame retardant toughening agent; The filler is prepared by compounding titanium dioxide, silicon micropowder and light calcium carbonate in a mass ratio of (10-12):(3-5):(3-4).
2. The flame-retardant high-insulation epoxy composite material according to claim 1, characterized in that: The accelerator is dimethylimidazole.
3. The flame-retardant high-insulation epoxy composite material according to claim 1, characterized in that: The defoamer is a polyoxyethylene polyoxypropanolamine ether defoamer.
4. The flame-retardant high-insulation epoxy composite material according to claim 1, characterized in that: The leveling agent is PV88 leveling agent.
5. A method for preparing the flame-retardant high-insulation epoxy composite material according to any one of claims 1 to 4, characterized in that: The steps include: Step (1) 70-90 parts of bisphenol A epoxy resin, 30-40 parts of filler, 2-3 parts of leveling agent, 2-3 parts of accelerator, 0.7-1.2 parts of defoamer and 5-8 parts of flame retardant toughening agent are added into a mixer for premixing, and then mixed and extruded by a twin-screw extruder, and after extrusion, cooled, tableted, crushed, ground and screened to obtain component A; component B is 6.5-8.5 parts of accelerated dicyandiamide curing agent; Step (2) Evenly mix component A and component B to obtain a flame retardant high insulation epoxy composite material.
6. The method for preparing the flame-retardant high-insulation epoxy composite material according to claim 5, characterized in that: The heating temperature of the extruder is 90-110° C.; the D50 particle size of the flame-retardant high-insulation epoxy composite material is 30-40 μm.
Citation Information
Patent Citations
Fast-cure epoxy powder composition
CN103059516A
Water-soluble polyurethane flame-retardant coating and preparation method thereof
CN104789106A