Method and device for separating iron from nickel-iron alloy
By roasting nickel ferroalloy under a chlorine atmosphere and carrying out chlorination reaction, the problem of long separation process of nickel ferroalloy is solved, and efficient and short-process preparation of ferrochloride is achieved, the process flow is simplified and the separation efficiency is improved.
Patent Information
- Application Number
- CN202410981328.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-22
Smart Images

Figure CN118497487B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of resource utilization, and in particular to a method and a device for separating iron from a nickel-iron alloy. Background Art
[0002] The efficient and fine separation of valuable elements in alloys and even waste alloys, such as copper-cobalt alloys and waste high-temperature alloys, has always been a difficult point in research. At present, the methods for resource utilization of waste alloys that have been studied include mechanical crushing, zinc melting, oxidation-reduction, electrochemical, and biological leaching. However, due to the stubborn properties of alloys, such as high hardness, density, corrosion resistance, and wear resistance, and the fact that most elements exist in the form of intermetallic compounds, most processes use metallurgical methods with three highs and one strong, resulting in long process flows, heavy environmental loads, and high energy consumption. It is urgent to develop short-process, high-efficiency, high-quality, and low-cost waste alloy processing technology.
[0003] The above-mentioned method for high-value utilization of nickel-iron alloy mainly involves first using reagents to wet-leach the nickel-iron alloy to destroy the dense structure of the nickel-iron alloy, while allowing nickel, iron, etc. in the alloy to enter the solution, and then the solution is purified and partially extracted for valuable metals. When the above-mentioned method leaches the nickel-iron alloy, both nickel and iron enter the leachate, which is not selective, which leads to subsequent lengthy extraction processes such as impurity removal and separation. Summary of the invention
[0004] The main purpose of the present invention is to provide a method and device for separating iron from nickel-iron alloy, so as to solve the technical problem that the leaching method has a long and multi-step process for separating nickel and iron.
[0005] To achieve the above object, the present invention provides a method for separating iron from nickel-iron alloy, comprising the following steps:
[0006] The nickel-iron alloy is roasted in a chlorine atmosphere to obtain a ferrous chloride melt and solid slag, and the ferrous chloride melt is separated, wherein the mass of the chlorine is 0.8 to 1.5 times the mass of the nickel-iron alloy, and the roasting temperature is 500 to 850°C.
[0007] Chlorine gas is introduced into the ferrous chloride melt to carry out a chlorination reaction, so that the ferrous chloride melt is converted into ferric chloride gas.
[0008] The ferric chloride gas is condensed to obtain a solid ferric chloride product.
[0009] According to an embodiment of the present application, in the step of introducing chlorine gas into the ferrous chloride melt for reaction, the chlorination temperature is 400-700° C., and the amount of chlorine gas introduced is 0.25-0.35 times the mass of the ferrous chloride melt.
[0010] According to an embodiment of the present application, in the step of condensing the ferric chloride gas, the ferric chloride gas is condensed to 100-250°C.
[0011] According to an embodiment of the present application, the chlorine gas is introduced into the bottom of the nickel-iron alloy for roasting.
[0012] The present application also provides a device for separating iron from nickel-iron alloy, comprising:
[0013] The roasting furnace comprises a furnace body and a first chlorine gas inlet, wherein the furnace body has a receiving cavity for receiving the nickel-iron alloy, the first chlorine gas inlet is connected to the receiving cavity, and the mass of the chlorine gas introduced is 0.8 to 1.5 times the mass of the nickel-iron alloy. The roasting temperature in the furnace body is 500 to 850°C.
[0014] A separation mechanism is communicated with the accommodating cavity and is used to separate the ferrous chloride melt generated by the furnace body.
[0015] The chlorination reaction chamber has a second chlorine gas inlet, and the chlorination reaction chamber is connected with the separation mechanism to receive the ferrous chloride melt.
[0016] The condensation mechanism is communicated with the chlorination reaction chamber and condenses the ferric chloride gas produced in the chlorination reaction chamber to produce a solid ferric chloride product.
[0017] The collecting mechanism is located below the condensing mechanism and collects the solid ferric chloride product.
[0018] According to an embodiment of the present application, the furnace body is cylindrical, and the ratio of the height to the diameter of the furnace body is (8-20): 1. The first chlorine gas inlet is located at the bottom of the furnace body. The temperature control component of the roasting furnace is located at 1 / 4-1 / 2 of the height of the furnace body measured from the bottom.
[0019] According to an embodiment of the present application, the separation mechanism includes a filter plate embedded in the bottom of the furnace body, and the pore size of the filter plate is 0.1~0.2mm.
[0020] The device for separating iron from nickel-iron alloy further comprises a melt collecting tank, which is connected to the furnace body and communicates with the accommodating cavity through the filter plate.
[0021] According to an embodiment of the present application, the chlorination reaction chamber is located below the furnace body.
[0022] The device for separating iron from nickel-iron alloy further comprises a communicating vessel. The diameter of the communicating vessel is 1 / 8 of the diameter of the furnace body. One end of the communicating vessel is connected to the melt collecting tank, and the other end is connected to the chlorination reaction chamber.
[0023] According to an embodiment of the present application, a side of the chlorination reaction chamber away from the communicating vessel has a gaseous ferric chloride ascending channel, and the gaseous ferric chloride ascending channel is connected to the condensing mechanism.
[0024] According to an embodiment of the present application, the collecting mechanism is a conical structure, and the diameter of the conical structure matches the bottom of the condensing mechanism.
[0025] Beneficial effects:
[0026] In the above-mentioned method for separating iron from nickel-iron alloy, by controlling the chlorination conditions, the preferential chlorination of iron in the alloy is achieved, and it is converted into molten ferrous chloride. Ferrous chloride is then converted into gaseous ferric chloride and volatilized, and ferric chloride is obtained by cooling. The element behavior of iron in the alloy is to change from solid alloy to liquid ferrous chloride, and then to gaseous ferric chloride, which realizes the continuity of the process. And in the process of molten ferrous chloride being gasified by chlorine, the reaction can be well controlled, and then high-quality ferric chloride can be prepared. The above-mentioned method for separating iron from nickel-iron alloy is simple to operate, has a short process flow, and obtains high-quality ferric chloride. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0028] Figure 1 is a flow chart of a method for separating iron from a nickel-iron alloy according to an embodiment of the present application;
[0029] Figure 2 It is a schematic structural diagram of a device for separating iron from nickel-iron alloy according to one embodiment of the present application.
[0030] Description of reference numerals: 100, roasting furnace; 200, separation mechanism; 300, chlorination reaction chamber; 400, condensation mechanism; 500, collection mechanism; 600, melt collection tank; 700, communicating vessel;
[0031] 110, furnace body; 120, feed assembly; 130, temperature control assembly; 140, slag outlet; 150, first chlorine gas inlet;
[0032] 310, chlorination oxidation reaction chamber; 320, gaseous ferric chloride ascending channel; 330, second chlorine gas inlet;
[0033] 410, condensation chamber; 420, temperature control component;
[0034] 510. Discharge switch. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0037] In addition, in the present invention, the descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0038] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0039] The present invention provides a method for separating iron from nickel-iron alloy, see Figure 1 , including the following steps:
[0040] S100: roasting the nickel-iron alloy in a chlorine atmosphere to obtain a ferrous chloride melt and solid slag, and separating the ferrous chloride melt, wherein the mass of the chlorine is 0.8 to 1.5 times the mass of the nickel-iron alloy, and the roasting temperature is 500 to 850°C.
[0041] The present invention provides a method for separating iron from a nickel-iron alloy, and the overall idea is as follows: by controlling the chlorination conditions, the preferential chlorination of iron in the alloy is achieved and converted into molten ferrous chloride. The unreacted nickel-iron alloy and the solid slag obtained by the reaction are both solid, and the molten ferrous chloride is liquid, which is easy to separate from the solid, such as by filtering, centrifugation, etc. Specifically in some embodiments, a filter hole is set at the bottom of the reaction container (such as a roasting furnace) of the nickel-iron alloy, so that the molten ferrous chloride is filtered out from the bottom of the container.
[0042] In the subsequent step, chlorine gas is introduced into the obtained molten ferrous chloride to convert the ferrous chloride into gaseous ferric chloride for volatilization. The gaseous ferric chloride is condensed to obtain a solid ferric chloride product, thereby completing the operation of separating iron from the nickel-iron alloy.
[0043] The nickel-iron alloy of the embodiment of the present application is an alloy whose main components are nickel and iron, and is a smelting intermediate. In some embodiments, the nickel-iron alloy of the embodiment of the present application is a nickel-iron alloy obtained by pyrometallurgical smelting of laterite nickel ore, such as a nickel-iron alloy obtained by RK-EF method, rotary kiln direct reduction-magnetic separation process, rotary hearth furnace-melting furnace process. In some specific embodiments, the composition of the nickel-iron alloy is shown in Table 1.
[0044] Table 1: Chemical composition of nickel-iron alloy (wt %)
[0045]
[0046] In step S100, the mass ratio of the quality of chlorine to the nickel-iron alloy and the roasting temperature are passed to achieve the preferential chlorination of iron in the alloy. When the roasting temperature and the chlorine content are too high, nickel and iron both generate chlorides, nickel generates gaseous nickel chloride, and iron generates gaseous ferrous chloride or gaseous ferric chloride, thereby failing to achieve the effect of solid-liquid separation. When the roasting temperature and the chlorine content are too low, the ferric chloride generated by iron is less or does not generate ferric chloride, and the effect of solid-liquid separation is equally failing to achieve.
[0047] The specific roasting time is not specifically required, and is based on the generation of ferrous chloride melt. In particular, in some embodiments, a continuous method for separating iron from ferronickel alloy is adopted. The total amount of ferronickel alloy is relatively large, and step S100 is a process of sustained reaction, in which ferronickel alloy is added in a large amount or continuously added to ferronickel alloy at one time, and in the roasting process, ferrous chloride melt and solid slag are continuously generated. As the reaction proceeds, the solid slag that the reaction is completed can also be separated.
[0048] In some specific embodiments, the mass of the chlorine gas is 0.8-1.5 times the mass of the nickel-iron alloy, and the calcination temperature is 600-800°C.
[0049] In step S100, possible reaction equations include:
[0050] Ni-Fe+Cl2(g)→FeCl2(l)+NiCl2(s)+Ni(s), FeCl2(l)+Cl2(g)→FeCl3(g), FeCl3(g)+Fe(s)→FeCl2(l); FeCl3(g)→Cl2(g)+FeCl2(g).
[0051] First, the present application controls the reaction conditions and adds a small amount of chlorine gas, so it is not easy for FeCl2 (l) to continue to react to generate FeCl3 (g).
[0052] Secondly, due to the small amount of chlorine added, the iron in the nickel-iron alloy is relatively excessive, and the excess iron continues to react with FeCl3 (g) to generate FeCl2 (l). FeCl2 (l) is continuously separated from the reaction system, which promotes the reaction to continue to generate FeCl2 (l) and consume FeCl3 (g).
[0053] Again, studies have shown that FeCl3 will decompose to form FeCl2+Cl2 at high temperatures (698K, i.e. 424.85°C). Thus, at some reaction temperatures in the present application, the formation of ferrous chloride is further promoted and FeCl3 (g) is consumed.
[0054] Therefore, under the influence of the above-mentioned factors, the main product in step S100 of the present application is FeCl2(l), i.e., molten ferric chloride, rather than ferric chloride.
[0055] In some more specific embodiments, the mass of the chlorine gas is 0.9-1.2 times the mass of the nickel-iron alloy, and the calcination temperature is 650-750°C.
[0056] S200: Chlorine gas is introduced into the ferrous chloride melt to carry out a chlorination reaction, so that the ferrous chloride melt is converted into ferric chloride gas.
[0057] In the process of molten ferrous chloride being gasified by chlorine, the reaction can be well controlled, and high-quality ferric chloride can be prepared. For example, ferrous chloride melt is placed in a chlorination reaction chamber, and chlorine is introduced into the molten ferrous chloride to cause a chlorination reaction between the two.
[0058] For example, if an iron-containing alloy is treated in one step to convert iron into ferric chloride, it is difficult to continue the one-step treatment. For example, when there is only a small amount of alloy in the later stage of the reaction, it is difficult for the introduced chlorine to contact the alloy, resulting in low utilization rate of chlorine.
[0059] After adopting the step-by-step treatment, one furnace is specifically responsible for the production of ferrous chloride, that is, when one batch of alloy has not yet completely reacted, the second batch of materials is added, and then the third batch of materials. The addition of materials can not only ensure the formation of ferrous chloride, but also ensure the contact efficiency between chlorine and alloy due to the high material content.
[0060] Moreover, after adopting the step-by-step method, the heat release of the reaction between ferrous chloride and chlorine is much lower than that of the reaction between chlorine and iron to generate ferrous chloride, and almost no heat is released. Therefore, the temperature of this step is easy to control, and the temperature can be controlled by using an external heat source.
[0061] In step S200, the reaction of Cl2(g)+FeCl2(g)→FeCl3(g) mainly occurs, which is the reverse reaction of the aforementioned FeCl3(g)→Cl2(g)+FeCl2(g). Therefore, in step S200, chlorine gas is introduced, which increases the concentration of reactants and moves the chemical equilibrium in the positive reaction direction, that is, in the direction of generating FeCl3(g).
[0062] In addition, during the chlorination process, iron is directly chlorinated into ferric chloride, which requires stronger chlorination conditions. See the analysis in part S100, which can easily lead to the chlorination of other elements in the alloy. In addition, during the chlorination process, iron is continuously volatilized, resulting in constantly changing reaction conditions, making it impossible to obtain relatively stable reaction conditions, which is not conducive to large-scale industrial production.
[0063] S300: Condensing the ferric chloride gas to obtain a solid ferric chloride product.
[0064] The boiling point of FeCl3 is 316℃. When the ferric chloride gas condenses below the boiling point, solid ferric chloride product is generated, which is easy to collect and store. During the entire separation process, the element behavior of iron in the alloy is to transform from solid alloy to liquid ferrous chloride, and then to gaseous ferric chloride, realizing the continuity of the process.
[0065] In the above-mentioned method for separating iron from nickel-iron alloy, by controlling the chlorination conditions, the preferential chlorination of iron in the alloy is achieved, and it is converted into molten ferrous chloride. Ferrous chloride is then converted into gaseous ferric chloride and volatilized, and ferric chloride is obtained by cooling. The element behavior of iron in the alloy is to change from solid alloy to liquid ferrous chloride, and then to gaseous ferric chloride, which realizes the continuity of the process. And in the process of molten ferrous chloride being gasified by chlorine, the reaction can be well controlled, and then high-quality ferric chloride can be prepared. The above-mentioned method for separating iron from nickel-iron alloy is simple to operate, has a short process flow, and obtains high-quality ferric chloride.
[0066] In some embodiments, in the step of introducing chlorine gas into the ferrous chloride melt for reaction, the chlorination temperature is 400-700° C., and the amount of chlorine gas introduced is 0.25-0.35 times the mass of the ferrous chloride melt.
[0067] Under this condition, the requirements for producing ferric chloride gas from ferrous chloride can be met, and the reaction degree is high.
[0068] The temperature of the ferrous chloride melt is relatively high. In some cases, the ferrous chloride melt can maintain a chlorination temperature of 400-700°C, such as a good insulation effect of the chlorination reaction vessel. In this case, no additional energy such as electric heating or gas combustion heating is required.
[0069] In other cases, the ferrous chloride melt cannot maintain the chlorination temperature of 400-700°C. In this case, additional energy such as electric heating or gas combustion heating is provided for assistance.
[0070] In some specific embodiments, the chlorination temperature is 400-700° C., and the amount of chlorine gas introduced is 0.25-0.35 times the mass of the ferrous chloride melt.
[0071] In some embodiments, in the step of condensing the ferric chloride gas, the ferric chloride gas is condensed to 100-250°C.
[0072] Under this condition, ferric chloride gas can be condensed into solid ferric chloride relatively quickly.
[0073] In some embodiments, the chlorine gas is introduced into the bottom of the nickel-iron alloy for roasting.
[0074] Since the density of chlorine is greater than that of air, the unreacted chlorine tends to stay at the bottom of the reaction vessel and is not likely to overflow upwards, causing waste of chlorine and environmental pollution.
[0075] Moreover, chlorine gas is introduced from the bottom of the nickel-iron alloy, and when the roasting and heating area is also at the bottom, ferrous chloride melt is generated at the bottom, so it is easy to separate. In addition, in this case, if the subsequent ferric chloride gas enters the device where the nickel-iron alloy is roasted, it will also react with the unreacted nickel-iron alloy above and be reduced to ferrous chloride melt.
[0076] The present application also provides a device for separating iron from nickel-iron alloy, see Figure 2 , including a roasting furnace 100, a separation mechanism 200, a chlorination reaction chamber 300, a condensation mechanism 400 and a collection mechanism 500.
[0077] The roasting furnace 100 includes a furnace body 110 and a first chlorine gas inlet 150. The furnace body 110 has a receiving cavity for receiving the nickel-iron alloy, and the first chlorine gas inlet 150 is connected to the receiving cavity, and the mass of the chlorine gas introduced is 0.8 to 1.5 times the mass of the nickel-iron alloy. The roasting temperature in the furnace body 110 is 500 to 850°C.
[0078] The specific shape of the roasting furnace 100 is not limited, such as cylindrical, square, etc.
[0079] In some embodiments, see Figure 2, the furnace body 110 is cylindrical, and the ratio of the height to the diameter of the furnace body 110 is (8-20): 1. In this case, the nickel-iron alloy raw material is piled high, and the height area of the nickel-iron alloy for chlorination reaction can be more accurately controlled, such as the chlorination reaction at the bottom of the roasting furnace 100 for roasting and heating. Referring to the beneficial effect of chlorine gas passing from the bottom of the nickel-iron alloy, it also has the effects of separating ferrous chloride melt, chlorine gas not escaping easily, and subsequent ferric chloride gas reduction into ferrous chloride melt. In addition, it is also beneficial for the iron in the alloy to continuously flow into the next reactor in the form of molten ferrous chloride.
[0080] In some embodiments, a feed assembly 120 is provided on the top of the furnace body 110 , such as a funnel-shaped structure.
[0081] In some embodiments, see Figure 2 There are two first chlorine gas inlets 150, which are located on both sides of the roasting furnace 100. In this embodiment, the first chlorine gas inlets 150 are symmetrically distributed, which is conducive to uniform distribution of chlorine.
[0082] In some embodiments, see Figure 2 The roasting furnace 100 further includes a temperature control component 130. Exemplarily, the temperature control component 130 is wrapped around the outside of the furnace body 110, and the wrapped height is 1 / 4 to 1 / 2 of the height of the furnace body 110. The temperature control component 130 is an electric temperature control component 130, which is realized by electric heating coupled with air condensation, that is, electric heating is turned on when the temperature is increased, and air condensation is turned on when the temperature is decreased.
[0083] The temperature control component 130 is arranged at the bottom, which is conducive to the nickel-iron alloy reaction starting from the bottom, so it has the effects of separating the ferrous chloride melt, preventing chlorine from escaping easily, and subsequently reducing the ferric chloride gas to the ferrous chloride melt.
[0084] In some embodiments, see Figure 2 The roasting furnace 100 further includes a slag outlet 140. The slag outlet 140 is located at 1 / 10 to 1 / 8 of the height of the furnace body 110 measured from the bottom. The solid slag obtained by the reaction is discharged from the slag outlet 140.
[0085] The separation mechanism 200 is communicated with the accommodating chamber to separate the ferrous chloride melt generated by the furnace body 110 .
[0086] The separation mechanism 200 may be provided integrally with the furnace body 110 or separately.
[0087] Taking an integrated configuration as an example, in some embodiments, the separation mechanism 200 includes a filter plate embedded in the bottom of the furnace body 110, and the pore size of the filter plate is 0.1-0.2 mm.
[0088] The filter plate is embedded in the furnace body 110, and its size is completely fitted with the bottom of the furnace body 110. The filter plate becomes a part of the bottom of the furnace body 110. The filter plate has filter holes. In this way, the ferrous chloride melt generated by the reaction flows directly through the filter holes to the next process. Exemplarily, the pore size of the filter plate is 0.1-0.2 mm.
[0089] In some embodiments, see Figure 2 The device for separating iron from nickel-iron alloy further includes a melt collecting tank 600, which is connected to the furnace body 110 and communicates with the accommodating cavity through the filter plate. The melt collecting tank 600 is located at the lower end of the filter plate and communicates with the filter plate. Exemplarily, the melt collecting tank 600 is in a cone shape. The upper opening of the melt collecting tank 600 matches and is fixedly connected to the bottom of the furnace body 110.
[0090] The chlorination reaction chamber 300 has a second chlorine gas inlet 330 . The chlorination reaction chamber 300 is communicated with the separation mechanism 200 to receive the ferrous chloride melt.
[0091] The condensation mechanism 400 is in communication with the chlorination reaction chamber 300, and condenses the ferric chloride gas generated in the chlorination reaction chamber 300 to produce a solid ferric chloride product.
[0092] The collecting mechanism 500 is located below the condensing mechanism 400 and collects the solid ferric chloride product.
[0093] The device for separating iron from nickel-iron alloy is used to implement the above-mentioned method for separating iron from nickel-iron alloy, and therefore has corresponding beneficial effects, which will not be described in detail. Its specific structure can be appropriately adjusted according to the implementation of different methods for separating iron.
[0094] In some embodiments, see Figure 2 The chlorination reaction chamber 300 includes a chlorination oxidation reaction chamber 310 and the aforementioned second chlorine gas inlet 330 .
[0095] Exemplarily, the chlorination oxidation reaction chamber 310 is a rectangular parallelepiped, such as length: width: height of 10:3:4 to 10:3:6. Exemplarily, the second chlorine gas inlet 330 is three chlorine gas inlet pipes, which are evenly distributed on the center line of the side, and the highest inlet pipe is distributed at 1 / 2 of the height of the chlorination oxidation reaction chamber 310 from the bottom of the chlorination oxidation reaction chamber 310, and the lowest inlet pipe is flush with the bottom of the chlorination oxidation reaction chamber 310. The second chlorine gas inlet 330 and the gaseous ferric chloride rising channel 320 are respectively distributed on both sides of the chlorination oxidation reaction chamber 310, and the second chlorine gas inlet 330 is located in the side lower measurement area of the chlorination oxidation reaction chamber 310 and is connected to the side.
[0096] In some embodiments, see Figure 2, the chlorination reaction chamber 300 is located below the furnace body 110. The device for separating iron from nickel-iron alloy further includes a connecting vessel 700. The diameter of the connecting vessel 700 is 1 / 8 of the diameter of the furnace body 110. One end (first end) of the connecting vessel 700 is connected to the melt collecting tank 600, and the other end (second end) of the connecting vessel 700 is connected to the chlorination reaction chamber 300.
[0097] The communicating vessel 700 is located below the furnace body 110. The ferrous chloride melt in the melt collecting tank 600 enters the second end from the first end of the communicating vessel 700 under the action of gravity, and then enters the chlorination oxidation reaction chamber 310. The second end is connected to the chlorination reaction chamber 300 through a pipeline such as an inverted L-shaped pipeline. In this way, the ferrous chloride melt exists at the bottom of the communicating vessel 700, which can play the role of a check valve, unidirectionally conducting, and only allowing the ferrous chloride melt to enter the chlorination reaction chamber 300. The gaseous ferric chloride generated in the chlorination reaction chamber 300 or the chlorine gas introduced therein cannot enter the melt collecting tank 600 and enter the furnace body 110 due to the presence of the ferrous chloride melt at the bottom of the communicating vessel 700. In some embodiments, the communicating vessel 700 is a U-shaped communicating vessel 700.
[0098] In some embodiments, see Figure 2 The chlorination reaction chamber 300 has a gaseous ferric chloride rising channel 320 on one side away from the communicating vessel 700 , and the gaseous ferric chloride rising channel 320 is connected to the condensing mechanism 400 .
[0099] Exemplarily, one end of the gaseous ferric chloride ascending channel 320 is located at the top of the chlorination oxidation reaction chamber 310 and communicated with the top, and the other end is communicated with the condensation mechanism 400. The second chlorine gas inlet 330 and the gaseous ferric chloride ascending channel 320 are respectively distributed on both sides of the chlorination oxidation reaction chamber 310.
[0100] Exemplarily, the gaseous ferric chloride ascending channel 320 is cylindrical, with a height of 1 / 3 to 1 / 2 of the furnace body 110 and a diameter of 1.1 to 1.2 times of the furnace body 110 .
[0101] In some embodiments, see Figure 2 The condensation mechanism 400 includes a condensation chamber 410 and a temperature control assembly 420. Exemplarily, the condensation mechanism 400 is cylindrical, with a height of 1 / 3 to 1 / 2 of the gaseous ferric chloride ascending channel 320 and a diameter of 5 to 10 times that of the gaseous ferric chloride ascending channel 320.
[0102] The temperature control component 420 is wrapped around the top and the outer sides of the condensation chamber 410, and the temperature is controlled by a water-cooled coupled heating rod for temperature regulation.
[0103] The collecting mechanism 500 is located at the bottom of the condensing mechanism 400 and is completely connected at the bottom. It is conical in shape. The diameter of the bottom of the cone is consistent with the condensing chamber 410. The height of the cone is 1.1 to 1.2 times that of the condensing chamber 410. The discharge switch 510 is located at the bottom of the collecting mechanism 500 and is connected to the collecting mechanism 500.
[0104] The technical solution of the present application is described below in conjunction with specific embodiments.
[0105] Embodiment 1:
[0106] use Figure 2 The device for separating iron from nickel-iron alloy shown in the figure processes the iron-containing alloy under the following conditions:
[0107] 10kg of nickel-iron alloy is added to the roasting furnace 100 at an average speed in 10 batches. After the first batch is added, chlorine is introduced into the roasting furnace 100 through the first chlorine gas inlet 150, and the amount of chlorine introduced is 1.2 times the mass of the nickel-iron alloy in the roasting furnace 100, and the roasting temperature is 650°C. After the ferrous chloride melt in the roasting furnace 100 flows into the chlorination reaction chamber 300, chlorine is introduced into the equipment through the second chlorine gas inlet 330, the chlorination temperature is 600°C, and the amount of chlorine introduced is 0.3 times the mass of ferrous chloride in the chlorination reaction chamber 300. The ferric chloride volatilized from the chlorination reaction chamber 300 flows into the condensation mechanism 400 for condensation collection, and the condensation temperature of the condensation mechanism 400 is controlled at 200°C. After the reaction is completed, the chlorinated slag in the roasting furnace 100 is detected and analyzed, indicating that the volatility of iron in the alloy is 92.74%. The ferric chloride product collected in the collecting mechanism 500 was tested, and the purity of the ferric chloride was 99.31%, and the content of ferrous chloride in the ferric chloride product was 0.05%.
[0108] Embodiment 2:
[0109] The reaction equipment is the same as that in Example 1.
[0110] The ferrous alloy was treated using the same apparatus as in Example 1 under the following conditions:
[0111] 10kg of nickel-iron alloy is added to the roasting furnace 100 at an average speed in 10 batches. After the first batch is added, chlorine is introduced into the device through the first chlorine gas inlet 150, and the amount of chlorine introduced is 1.2 times the mass of the nickel-iron alloy in the roasting furnace 100 and the roasting temperature is 600°C. After the ferrous chloride melt in the roasting furnace 100 flows into the chlorination reaction chamber 300, chlorine is introduced into the device through the second chlorine gas inlet 330, the chlorination temperature is 600°C, and the amount of chlorine introduced is 0.3 times the mass of ferrous chloride in the chlorination reaction chamber 300. The ferric chloride volatilized from the chlorination reaction chamber 300 flows into the condensation mechanism 400 for condensation collection, and the condensation temperature of the condensation mechanism 400 is controlled at 100°C. After the reaction is completed, the chlorinated slag in the roasting furnace 100 is detected and analyzed, indicating that the volatility of iron in the alloy is 87.51%. The ferric chloride product collected in the collecting mechanism 500 was tested, and the purity of the ferric chloride was 99.84%, and the content of ferrous chloride in the ferric chloride product was 0.03%.
[0112] Embodiment 3:
[0113] The reaction equipment is the same as that in Example 1.
[0114] The ferrous alloy was treated using the same apparatus as in Example 1 under the following conditions:
[0115] 10kg of nickel-iron alloy is added to the roasting furnace 100 at an average speed in 10 batches. After the first batch is added, chlorine is introduced into the device through the first chlorine gas inlet 150, and the amount of chlorine introduced is 1.4 times the mass of the nickel-iron alloy in the roasting furnace 100 and the roasting temperature is 850°C. After the ferrous chloride melt in the roasting furnace 100 flows into the chlorination reaction chamber 300, chlorine is introduced into the device through the second chlorine gas inlet 330, the chlorination temperature is 650°C, and the amount of chlorine introduced is 0.4 times the mass of ferrous chloride in the chlorination reaction chamber 300. The ferric chloride volatilized from the chlorination reaction chamber 300 flows into the condensation mechanism 400 for condensation collection, and the condensation temperature of the condensation mechanism 400 is controlled at 100°C. After the reaction is completed, the chlorinated slag in the roasting furnace 100 is detected and analyzed, indicating that the volatility of iron in the alloy is 97.49%. The ferric chloride product collected in the collecting mechanism 500 was tested, and the purity of the ferric chloride was 98.94%, and the content of ferrous chloride in the ferric chloride product was 0.01%.
[0116] Comparative Example 1:
[0117] 1kg of nickel-iron alloy was added into a horizontal tube furnace (quartz tube was used as furnace tube), the amount of chlorine gas introduced was 1.8 times the mass of nickel-iron alloy in the horizontal tube furnace, and the roasting temperature was 650℃, so that the iron in the alloy was directly volatilized (stop after no obvious volatiles were produced in the reaction zone), and then the volatile gas phase was condensed, and the condensation temperature was controlled at 100℃. The chlorinated slag in the chlorination furnace was analyzed and tested, indicating that the chlorination volatilization rate of the iron in the alloy was 47.9%. The collected ferric chloride product was tested, and the purity of ferric chloride was 95.01%, and the ferrous chloride content in the ferric chloride product was 4.72%.
[0118] Comparative Example 2:
[0119] 1kg of nickel-iron alloy was added into a horizontal tube furnace (quartz tube was used as furnace tube), the amount of chlorine gas introduced was 3.5 times the mass of nickel-iron alloy in the horizontal tube furnace, and the roasting temperature was 650℃, so that the iron in the alloy was directly volatilized (stop after no obvious volatiles were produced in the reaction zone), and then the volatile gas phase was condensed, and the condensation temperature was controlled at 100℃. The chlorinated slag in the chlorination furnace was analyzed and tested, indicating that the chlorination volatilization rate of iron in the alloy was 87.49%. The collected ferric chloride product was tested, and the purity of ferric chloride was 97.90%, and the content of ferrous chloride in the ferric chloride product was 1.94%.
[0120] Comparative Example 3:
[0121] 1kg of nickel-iron alloy was added into a horizontal tube furnace (quartz tube was used as furnace tube), the amount of chlorine gas introduced was 3.5 times the mass of nickel-iron alloy in the horizontal tube furnace, and the roasting temperature was 450℃, so that the iron in the alloy was directly volatilized (stop after no obvious volatiles were produced in the reaction zone), and then the volatile gas phase was condensed, and the condensation temperature was controlled at 100℃. The chlorinated slag in the chlorination furnace was analyzed and tested, indicating that the chlorination volatilization rate of the iron in the alloy was 45.79%. The collected ferric chloride product was tested, and the purity of ferric chloride was 99.31%, and the content of ferrous chloride in the ferric chloride product was 0.74%.
[0122] Comparative Example 4:
[0123] The reaction equipment is the same as that in Example 1.
[0124] The ferrous alloy was treated using the same apparatus as in Example 1 under the following conditions:
[0125] 10kg of nickel-iron alloy is added to the roasting furnace 100 at a uniform speed in 10 batches. After the first batch is added, chlorine is introduced into the device through the first chlorine gas inlet 150, and the amount of chlorine is 0.75 times the mass of the nickel-iron alloy in the roasting furnace 100 and the roasting temperature is 650°C. After the ferrous chloride melt in the roasting furnace 100 flows into the chlorination reaction chamber 300, chlorine is introduced into the device through the second chlorine gas inlet 330, the chlorination temperature is 650°C, and the amount of chlorine is 0.3 times the mass of ferrous chloride in the chlorination reaction chamber 300. The ferric chloride volatilized from the chlorination reaction chamber 300 flows into the condensation mechanism 400 for condensation collection, and the condensation temperature of the condensation mechanism 400 is controlled at 100°C. After the reaction is completed, the chlorinated slag in the roasting furnace 100 is detected and analyzed, indicating that the volatility of iron in the alloy is 69.07%. The ferric chloride product collected in the collecting mechanism 500 was tested, and the purity of the ferric chloride was 98.95%, and the content of ferrous chloride in the ferric chloride product was 0.09%.
[0126] Comparing Comparative Examples 1 to 4 and each embodiment, it is not easy to continuously pass the nickel-iron alloy into Comparative Example 1 due to the adoption of a horizontal tube furnace, and the furnace tube of the horizontal tube furnace is arranged horizontally, and the height of its vertical space is shorter, so the nickel-iron alloy material is shorter, and chlorine is also easily overflowed laterally along the furnace tube, so the chlorine utilization rate is relatively low. When more chlorine is passed than in the embodiment, the chlorination volatility of the iron of the alloy is still relatively low. Until Comparative Example 2 is passed into the chlorine intake of several times of the embodiment, the chlorination volatility substantially similar to the embodiment is reached. And the ferrous chloride content in the ferric chloride product obtained by the comparative example is significantly higher than the ferric chloride product obtained in the embodiment.
[0127] In Comparative Example 3, due to the low calcination temperature and the use of a horizontal tube furnace, even if a large amount of chlorine gas is introduced, the chlorination volatilization rate of iron in the alloy is still low. In addition, the ferrous chloride content in the ferric chloride product obtained in Comparative Example 3 is significantly higher than that in the ferric chloride product obtained in the example.
[0128] In Comparative Example 4, since the amount of chlorine introduced is too low, the chlorination volatilization rate of the iron in the alloy is still relatively low.
[0129] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for separating iron from nickel-iron alloy, characterized in that: The following steps are involved: The nickel-iron alloy is roasted in a chlorine atmosphere to obtain a ferrous chloride melt and solid slag, and the ferrous chloride melt is separated; wherein the mass of the chlorine is 0.8 to 1.5 times the mass of the nickel-iron alloy, and the roasting temperature is 600 to 850° C.; Chlorine gas is introduced into the ferrous chloride melt to carry out a chlorination reaction, so that the ferrous chloride melt is converted into ferric chloride gas; wherein the chlorination temperature is 400-700° C., and the amount of chlorine gas introduced is 0.25-0.35 times the mass of the ferrous chloride melt; The ferric chloride gas is condensed to obtain a solid ferric chloride product.
2. The method for separating iron from nickel-iron alloy according to claim 1, characterized in that: In the step of condensing the ferric chloride gas, the ferric chloride gas is condensed to 100-250°C.
3. The method for separating iron from nickel-iron alloy according to claim 1 or 2, characterized in that: The chlorine gas is introduced into the bottom of the nickel-iron alloy for roasting.
4. The method for separating iron from nickel-iron alloy according to claim 1, characterized in that: The device for implementing the method of separating iron from nickel-iron alloy comprises: A roasting furnace, comprising a furnace body and a first chlorine gas inlet, wherein the furnace body has a containing cavity for containing the nickel-iron alloy, the first chlorine gas inlet is connected to the containing cavity, and the mass of the introduced chlorine gas is 0.8 to 1.5 times the mass of the nickel-iron alloy; the roasting temperature in the furnace body is 600 to 850°C; A separation mechanism, connected to the accommodating chamber, for separating the ferrous chloride melt generated by the furnace body; a chlorination reaction chamber having a second chlorine gas inlet, the chlorination reaction chamber being in communication with the separation mechanism and receiving the ferrous chloride melt; a condensing mechanism, which is in communication with the chlorination reaction chamber and condenses the ferric chloride gas produced in the chlorination reaction chamber to produce a solid ferric chloride product; The collecting mechanism is located below the condensing mechanism and collects the solid ferric chloride product.
5. The method for separating iron from nickel-iron alloy according to claim 4, characterized in that: The furnace body is cylindrical, and the ratio of the height to the diameter of the furnace body is (8~20):1; the first chlorine gas inlet is located at the bottom of the furnace body; the temperature control component of the roasting furnace is located at 1 / 4~1 / 2 of the height of the furnace body measured from the bottom.
6. The method for separating iron from nickel-iron alloy according to claim 4, characterized in that: The separation mechanism comprises a filter plate embedded in the bottom of the furnace body, and the pore size of the filter plate is 0.1-0.2 mm; The device for separating iron from nickel-iron alloy further comprises a melt collecting tank, which is connected to the furnace body and communicates with the accommodating cavity through the filter plate.
7. The method for separating iron from nickel-iron alloy according to claim 6, characterized in that: The chlorination reaction chamber is located below the furnace body; The device for separating iron from nickel-iron alloy also includes a communicating vessel; the diameter of the communicating vessel is 1 / 8 of the diameter of the furnace body; one end of the communicating vessel is connected to the melt collecting tank, and the other end is connected to the chlorination reaction chamber.
8. The method for separating iron from nickel-iron alloy according to claim 7, characterized in that: A gaseous ferric chloride ascending passage is provided on a side of the chlorination reaction chamber away from the communicating vessel, and the gaseous ferric chloride ascending passage is communicated with the condensing mechanism.
9. The method for separating iron from nickel-iron alloy according to claim 7, characterized in that: The collecting mechanism is a conical structure, and the diameter of the conical structure matches the bottom of the condensing mechanism.
Citation Information
Cited By
Iron-nickel alloy high-temperature chlorination separation system and method
CN120193156A
Method and device for separating ferro-nickel-containing alloy through low-temperature chlorination
CN120591548A
Iron-nickel alloy high-temperature chlorination separation system
CN224199434U