A method for purifying and removing impurities from waste lithium iron phosphate powder
By using specific chelating resin extractants in a step-by-step process to treat waste lithium iron phosphate powder, the problem of removing titanium, aluminum, and copper impurities during the recycling process has been solved, achieving efficient separation and low-cost purification of lithium iron phosphate powder, thus improving the quality of recycled products.
Patent Information
- Application Number
- CN202410726592.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-06-06
AI Technical Summary
Existing technologies struggle to effectively remove impurities such as titanium, aluminum, and copper when recycling used lithium iron phosphate batteries, affecting the uniformity and stability of the recycled products.
Using chelating resins with specific structures as extractants A and B, the leachate of waste lithium iron phosphate powder was extracted in steps to remove copper, titanium, and aluminum respectively. Back-extraction and washing were performed using an acidic solution to prepare battery-grade lithium iron phosphate and lithium carbonate.
It achieves efficient separation of copper, titanium and aluminum, reduces impurity content, and the resulting raffinate can be used to prepare high-quality battery-grade iron phosphate and lithium carbonate. The operation is simple and low-cost.
Smart Images

Figure SMS_46 
Figure SMS_47 
Figure SMS_48
Abstract
Description
Technical Field
[0001] This invention relates to the field of hydrometallurgical technology. Specifically, this invention relates to a method for purifying and removing impurities from waste lithium iron phosphate powder. Background Technology
[0002] With the rapid development of hybrid electric vehicles and electric vehicles, the production of power lithium-ion batteries has increased significantly. When power lithium-ion batteries reach the end of their lifespan, a large number of waste power lithium-ion batteries will inevitably be generated.
[0003] Methods for preparing battery-grade iron phosphate using wet processes to recycle waste lithium iron phosphate cathode materials generally face the challenge of high impurity content. Furthermore, without targeted and in-depth removal of titanium, aluminum, and copper during large-scale lithium iron phosphate battery recycling, the uniformity and stability of the recycled iron phosphate product's quality will also be affected. In-depth removal of metallic impurities has significant research value and practical implications.
[0004] A method for preparing lithium iron phosphate cathode material from spent lithium iron phosphate batteries exists in this field. The specific production steps are as follows: acid leaching, copper removal, aluminum removal, preparation of iron phosphate dihydrate, lithium precipitation, and preparation of lithium carbonate. Although this method achieves full component recovery of spent lithium iron phosphate battery material, the impurity content in the obtained iron phosphate dihydrate still needs to be further reduced.
[0005] How to effectively remove titanium, aluminum, and copper from lithium iron phosphate battery waste liquid has become an urgent problem that the lithium battery industry needs to solve. Summary of the Invention
[0006] Therefore, one object of the present invention is to effectively remove titanium, aluminum and copper from waste lithium iron phosphate powder.
[0007] The above-mentioned objectives of the present invention can be achieved through the following technical solutions: A method for purifying and removing impurities from waste lithium iron phosphate powder, characterized by comprising: S1: Use an acidic solution to leach waste lithium iron phosphate powder to obtain a leachate containing iron, aluminum, titanium and copper; S2: Extract the leachate with extractant A to remove copper, and obtain copper-free raffinate A and copper-loaded extractant A; S3: Extract the copper-removed raffinate A with extractant B to remove titanium and aluminum, obtaining titanium and aluminum-removed raffinate B and titanium and aluminum-loaded extractant B. in, The extractant A comprises a chelating resin having the structure shown in Formula I: Formula I in: M is the resin matrix. R1 and R2 are each independently hydrogen and -(CH2). q -C(O)R5, where R1 and R2 are not both hydrogen, and R5 is selected from any one or two C1-C bonds. 10 An alkyl or alkenyl-substituted amino group, wherein the alkyl or alkenyl group is optionally substituted with a halogen; The extractant B comprises a chelating resin having the structure shown in Formula II: Formula II in: M is the resin matrix. R3 and R4 are each independently selected from hydrogen, -CH2-P(O)(R6)2, and -CHR8-(CH2). t -COR7, and at least one of R3 and R4 is -CH2-P(O)(R6)2. R6 is selected from -OH, -ONa, -OK, and optionally halogenated C1-C. 10 Alkoxy R7 is selected from hydroxyl groups, optionally halogenated C1-C. 10 Alkyl groups and optionally one or both C1-C 10 An alkyl or alkenyl-substituted amino group, wherein the alkyl or alkenyl group is optionally substituted with a halogen. R8 is selected from hydrogen, or optionally halogenated C1-C. 10 Alkyl groups and phenyl groups optionally substituted with C1-C4 alkyl groups or halogens, q is any integer from 1 to 4. t is 0 or 1.
[0008] The method of this invention has high extraction efficiency for copper, aluminum and titanium impurities, resulting in good separation of copper, titanium and aluminum. The obtained raffinate can be used to prepare battery-grade iron phosphate, lithium carbonate or lithium iron phosphate. Detailed Implementation
[0009] The various aspects of the invention, as well as further objects, features and advantages, will be set forth more fully below.
[0010] The method of the present invention is based on the inventors’ discovery that the chelating resin having the structure shown in Formula I has high extraction efficiency for copper, but low extraction efficiency for iron and aluminum, thereby enabling the separation of copper from iron and aluminum.
[0011] The method of the present invention can effectively remove copper from the leachate while retaining aluminum and iron.
[0012] The inventors also discovered that the chelating resin with the structure shown in Formula I has low extraction efficiency for titanium, thereby enabling effective separation of copper and titanium.
[0013] Preferably, the acid in the acidic solution in step S1 is sulfuric acid.
[0014] More preferably, the leaching process includes preparing a slurry of waste lithium iron phosphate powder and a leaching agent, followed by the addition of concentrated sulfuric acid for a first-stage leaching, yielding a first-stage leaching residue and a first-stage leaching solution. Preferably, the concentrated sulfuric acid has a mass concentration of 90% or higher, for example, 98%.
[0015] Preferably, a section of the leaching solution is directly introduced into step S2 to remove copper.
[0016] Preferably, the first-stage leaching residue is subjected to second-stage leaching, that is, the first-stage leaching residue and leaching agent are mixed into a slurry, and then concentrated sulfuric acid is added for second-stage leaching to obtain second-stage leaching residue and second-stage leachate.
[0017] In this application, when “leaching” is mentioned, it may refer to primary leaching, secondary leaching, or both.
[0018] Preferably, before step S2, the pH of the leachate is adjusted to 0.5-4.5, more preferably 0.5-3.
[0019] In some implementations, the pH of the leachate is adjusted using an alkaline solution and / or waste lithium iron phosphate powder.
[0020] The alkaline solution can be sodium hydroxide, potassium hydroxide, or ammonia, with ammonia being the preferred option.
[0021] Preferably, waste lithium iron phosphate powder is used to adjust the pH of the leachate, and solid-liquid separation is performed to obtain a leachate containing iron, aluminum, titanium and copper and leach residue 1.
[0022] Preferably, the leaching residue 1 is returned to the second stage of leaching.
[0023] Optionally, the second-stage leaching residue is washed with water to obtain washed leaching residue and washing water. Preferably, the washing water is returned to the first-stage or second-stage leaching reactor.
[0024] Furthermore, the leaching agent includes water, the washing water of the second-stage leaching residue, or a mixture of both.
[0025] Preferably, the leaching agent is water.
[0026] In this application, when “water” is referred to, it means pure water, unless the context leads to the opposite interpretation.
[0027] Preferably, the liquid-to-solid volume / mass (mL / g) ratio during leaching is 1.5-5:1, more preferably 3-5:1.
[0028] Preferably, the acid mass concentration during leaching is 15%-50%, more preferably 15%-30%.
[0029] Preferably, the leaching duration is 1-5 h, more preferably 2-3 h.
[0030] Preferably, the leaching is carried out at a temperature of 40°C-100°C, more preferably 60-90°C.
[0031] This invention does not specifically limit the base resin M in Formula I and Formula II.
[0032] Preferably, in Formula I and Formula II, the resin matrix M is independently selected from polystyrene resin, copolymer of styrene and divinylbenzene, phenolic resin polymer, polyacrylic resin or silicone resin.
[0033] More preferably, the resin matrix M is independently selected from polystyrene resin or copolymer of styrene and divinylbenzene.
[0034] As used in this article, "halogenated" means that at least one hydrogen atom is replaced by a halogen.
[0035] As used in this article, "halogen" refers to fluorine, chlorine, bromine, or iodine.
[0036] Preferably, R5 is selected from amino groups optionally substituted with one or two C1-C6 alkyl groups.
[0037] More preferably, R5 is selected from amino groups optionally substituted with one or two C1-C4 alkyl groups.
[0038] More preferably, R5 is selected from the following groups: , , , , , , in This is the connection site.
[0039] Advantageously, when R3 is different from R4, R6 is selected from -OH, -ONa and -OK.
[0040] Preferably, R7 is selected from hydroxyl, optionally halogenated C1-C4 alkoxy, and optionally substituted amino groups with one or two C1-C6 alkyl groups.
[0041] More preferably, R7 is selected from hydroxyl groups and amino groups optionally substituted with one or two C1-C4 alkyl groups.
[0042] Preferably, R8 is selected from hydrogen, optionally halogenated C1-C4 alkyl and phenyl groups, and more preferably hydrogen.
[0043] Preferably, q is 1 or 2. Preferably, t is 0 Preferably, the chelating resin having the structure of Formula I is selected from the following structures: , , , , , , , , , , , Preferably, the chelating resin having the structure of Formula II is selected from the following structures: , , , , , , , , , , , , , , More preferably, the chelating resin having the structure of Formula II is selected from the following structures: , , , , , , , M is independently selected from polystyrene resins and copolymers of styrene and divinylbenzene.
[0044] Preferably, the extractant A and extractant B are pretreated with an alkaline solution for neutralization and transformation before extraction.
[0045] For example, the alkaline solution can be a sodium hydroxide solution, a potassium hydroxide solution, ammonia, a sodium carbonate solution, or a potassium carbonate solution, with ammonia being preferred.
[0046] The neutralization and transformation pretreatment can be performed multiple times or cyclically.
[0047] Extraction can be performed on one or more columns, such as 1 to 10 columns.
[0048] In the case of multi-column extraction, the extractant used in each column can be the same or different.
[0049] Furthermore, the method includes a first back-extraction of the copper-loaded extractant A to obtain a copper-rich solution.
[0050] Furthermore, the method includes a second back-extraction of the titanium-aluminum loaded extractant B to obtain a second back-extraction solution.
[0051] Preferably, the first and second back-extractions are performed using an acid solution. Preferably, the acid solution used for back-extraction is selected from sulfuric acid solution and hydrochloric acid solution, with sulfuric acid solution being preferred. Preferably, the concentration of the acid solution used for back-extraction is 0.5-6 mol / L, with 0.5-3 mol / L being more preferred.
[0052] Furthermore, the acid solution used for the second back-extraction also contains hydrogen peroxide. Preferably, the molar ratio of hydrogen peroxide to titanium in the second back-extraction solution is 0.1-10, more preferably 1.5-3.
[0053] Preferably, washing is performed before the first and second back-extraction processes.
[0054] The washing is performed using a washing solution selected from water or an acid solution. Preferably, the pH value of the acid solution used for washing is 0-3.
[0055] Preferably, the acid solution used for washing is selected from hydrochloric acid solution and sulfuric acid solution, more preferably sulfuric acid solution.
[0056] The back-extraction can be performed once or more.
[0057] In some implementations, the back-extraction is performed twice.
[0058] Preferably, the method further includes preparing iron phosphate, lithium carbonate, or lithium iron phosphate using the raffinate B after removing titanium and aluminum.
[0059] The chelating resin of formula I mentioned in this application can be prepared by a preparation method including the following steps: The chelated resin is obtained by substituting the primary amine group of a primary amine resin with a halogenated derivative of formula IA. (Formula IA), in: R5 is as defined for equation I; X = Cl, Br, or I; q is as defined for equation I. A primary amine resin is a resin having primary amine groups on a resin matrix, wherein the resin matrix is as defined with respect to Formula I.
[0060] The primary amine resin can be pretreated before the substitution reaction.
[0061] Specifically, the pretreatment includes rinsing the primary amine resin with a solvent, stirring and shaking the primary amine resin, and then removing excess solvent.
[0062] Preferably, the solvent used in the pretreatment is a mixture of one or more solvents selected from water, ethanol, diethyl ether, toluene, dioxane, N,N-dimethylformamide, dichloromethane, and ethyl acetate.
[0063] Preferably, the substitution reaction is carried out in an alkaline solution at a temperature of 40-120°C.
[0064] Preferably, the solute in the alkaline solution during the substitution reaction is one or a combination of two or more of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, ammonia, and calcium hydroxide.
[0065] Preferably, the solvent of the alkaline solution in the substitution reaction is one or a combination of two or more of water, ethanol, methanol, and N,N-dimethylformamide.
[0066] Preferably, the ratio of the amount of solute in the alkaline solution during the substitution reaction to the molar amount of the primary amine group in the resin is 0.8-2.5:1.
[0067] Preferably, the ratio of the primary amine group content of the primary amine resin to the molar amount of the halogenated derivative of formula IA is 1:1-4, more preferably 1:1.5-3.5.
[0068] Preferably, the amount of solvent used is 1-30 times the mass of the resin.
[0069] Preferably, the reaction time in the substitution reaction is 4-48 hours.
[0070] The chelating resin of formula II mentioned in this application can be prepared by a preparation method including the following steps: 1) The primary amine group of the primary amine resin is substituted with a halocarboxylic acid of formula IIA or its derivative to obtain an intermediate resin. (Formula IIA) in: t is as defined for Equation II; R7 is as defined for Equation II; R8 is as defined for Equation II; X = Cl, Br, or I; and 2) The obtained intermediate resin is reacted with the phosphorus-containing substance of Formula III in an acidic solution in the presence of formaldehyde at a temperature of 40-120°C to obtain the chelated resin having the structure shown in Formula II. (Formula III) Where R6 is as defined for Equation II; or a) In an acidic solution in the presence of formaldehyde, a primary amine resin is reacted directly with a phosphorus-containing substance of Formula III as described above at a temperature of 40-120°C to obtain the chelating resin having the structure shown in Formula II.
[0071] Before step 1) or step a), the resin matrix may be pretreated as described above.
[0072] Preferably, the reaction in step 1) is carried out in an alkaline solution at a temperature of 40-120°C.
[0073] Preferably, the solute in the alkaline solution in step 1) is one or a combination of two or more of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, ammonia, and calcium hydroxide.
[0074] Preferably, the solvent of the alkaline solution in step 1) is one or a combination of two or more of water, ethanol, methanol, and N,N-dimethylformamide.
[0075] Preferably, the ratio of the amount of solute in the alkaline solution in step 1) to the molar amount of primary amine groups in the resin is 0.8-2.5:1.
[0076] Preferably, the ratio of the primary amine group content of the resin to the molar amount of the halogenated carboxylic acid or its derivative of formula IIA is 1:0.75-1.75, more preferably 1:0.8-1.5.
[0077] Preferably, the amount of solvent used in the alkaline solution in step 1) is 1-30 times the mass of the resin.
[0078] Preferably, the reaction time in step 1) is 4-48 hours.
[0079] Preferably, in step 2) or step a), the acid in the acidic solution is one or more of sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, and perchloric acid.
[0080] Preferably, in step 2) or step a), the solvent in the acidic solution is one or a mixture of water, ethanol, methanol, and N,N-dimethylformamide.
[0081] Preferably, the concentration of the acidic solution is 0.1-6 mol / L.
[0082] Preferably, in step 2), the molar ratio of the primary amine group of the resin matrix, formaldehyde and phosphorus-containing substance of formula III is 1:1-1.5:0.75-1.75, more preferably 1:1-1.25:0.8-1.5.
[0083] Preferably, in step a), the molar ratio of the primary amine group of the resin matrix, formaldehyde and phosphorus-containing substance of formula III is 1:1-3:0.75-3.5, more preferably 1:1-2.5:0.8-3.
[0084] Preferably, the amount of solvent in the acidic solution is 1-30 times the mass of the resin.
[0085] Preferably, in step 2) or step a), the reaction time is 4-48 hours.
[0086] The above preparation method can effectively prepare the chelating resin with the structure shown in Formula II of this application.
[0087] The method of this invention can efficiently extract copper, titanium and aluminum, with a removal rate of up to 98%.
[0088] Furthermore, the method for purifying and removing impurities from waste lithium iron phosphate powder provided by this invention has good separation effect on aluminum, titanium and copper, is simple to operate, has low process cost, low phosphorus and iron loss rate, and the obtained raffinate can be used to prepare battery-grade lithium iron phosphate, lithium carbonate or lithium iron phosphate.
[0089] Furthermore, the resin used in the method for purifying and removing impurities from waste lithium iron phosphate powder provided by this invention can be reused after back-extraction and regeneration, resulting in low operating costs and good economic benefits.
[0090] In this application, the term "and / or" covers situations involving one or both of the mentioned elements.
[0091] In this application, the terms "comprising" and "including" cover situations where other elements not explicitly mentioned are also included, as well as situations where the mentioned elements constitute the entirety of the application.
[0092] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In the event of any discrepancy between the definitions of terms in this specification and their commonly understood meaning by one of ordinary skill in the art to which this invention pertains, the definitions set forth herein shall prevail.
[0093] Unless otherwise stated, all numerical values for the amount of ingredients, temperature, time, etc., used in the specification and claims are to be understood as being modified by the term "about". Therefore, unless otherwise indicated, the numerical parameters set forth herein are approximate values that can be varied to obtain the desired performance.
[0094] Example The following will further illustrate the concept, specific structure, and technical effects of the present invention with reference to embodiments, so as to enable those skilled in the art to fully understand the purpose, features, and effects of the present invention. It will be readily understood by those skilled in the art that the embodiments described herein are merely illustrative, and the scope of the present invention is not limited thereto.
[0095] Synthesis Example 1 Resin 1 was prepared according to the following synthetic route: Specifically, 10 g (30 mmol, -NH2) primary amine polystyrene resin (from Samsung Resin, model SX382), 9.76 g (72 mmol) 2-chloro-N-ethyl-N-methylacetamide and 7.6 g (72 mmol) sodium carbonate were placed in a 100 ml three-necked flask, and 50 ml LDMF (N,N-dimethylformamide) was added. The mixture was heated at 80 °C for 12 hours under mechanical stirring to obtain resin 1.
[0096] Synthesis Example 2 Resin 2 was prepared according to the following synthetic route: Specifically, 10 g (30 mmol, -NH2) primary amine polystyrene resin (from Samsung Resin, model SX382), 8.75 g (72 mmol) 2-chloro-N,N-dimethylacetamide and 2.88 g (72 mmol) sodium hydroxide were placed in a 100 ml three-necked flask, and 50 mL of N,N-dimethylformamide was added. The mixture was heated at 80 °C for 12 hours under mechanical stirring to obtain resin 2.
[0097] Synthesis Example 3 Resin 3 was prepared according to the following synthetic route: Take 10 g (30 mmol, -NH2) primary amine polystyrene resin (from Samsung Resin, model SX382) into a 100 ml three-necked flask, then add 3 mL (30 mmol) formaldehyde solution and 2.45 g (30 mmol) phosphorous acid, and add 70 mL 0.5 mol / L sulfuric acid solution. Under mechanical stirring, react at 100 °C for 24 hours to obtain resin 3.
[0098] Synthesis Example 4 Resin 4 was prepared according to the following synthetic route: Take 10 g (30 mmol, -NH2) primary amine polystyrene resin (from Samsung Resin, model SX382), 3.3 g (35 mmol) chloroacetic acid and 3.7 g (35 mmol) sodium carbonate into a 100 ml three-necked flask, add 50 mL of water, and heat at 80 °C for 12 hours under mechanical stirring to obtain intermediate resin 4.
[0099] Next, 3 mL (30 mmol) of formaldehyde solution and 2.45 g (30 mmol) of phosphorous acid were added to intermediate resin 4, along with 70 mL of 0.5 mol / L sulfuric acid solution. The mixture was then reacted at 100 °C for 24 hours under mechanical stirring to obtain resin 4.
[0100] Synthesis Example 5 Resin 5 was prepared according to the following synthetic route: Take 10 g (30 mmol, -NH2) primary amine polystyrene resin (from Samsung Resin, model SX382) into a 100 ml three-necked flask, then add 6 mL (60 mmol) formaldehyde solution and 8.3 g (60 mmol) diethyl phosphite, add 70 mL 1 mol / L sulfuric acid solution, and react at 100 °C for 24 hours under mechanical stirring to obtain resin 5.
[0101] Example 1 Leaching Using lithium iron phosphate battery powder as raw material, the main element contents (by mass) are as follows: Al 0.54%, Cu 0.48%, Fe 32.23%, P 19.34%, Li 4.14%, Ti 0.17%.
[0102] Lithium iron phosphate battery powder (0.5 kg) was added to the reactor, and 2 L of pure water was added at a liquid-to-solid volume ratio of 4 mL:1 g to prepare the slurry. Then, 98% concentrated sulfuric acid (0.3 L) was added for a first-stage leaching. The acid leaching temperature was controlled at 80℃ and the reaction was carried out for 1.5 h. After the leaching was completed, the first-stage leachate and the first-stage leachate residue were obtained by filtration.
[0103] First-stage leaching residue and 2L of pure water were added to the reactor for slurry preparation. Then, 0.3L of 98% concentrated sulfuric acid was added for second-stage leaching. The acid leaching temperature was controlled at 85℃ and the reaction was carried out for 2 hours. After leaching, the second-stage leaching solution and second-stage leaching residue were obtained by filtration. The second-stage leaching residue was washed three times with water, with 0.8L of water used each time, to obtain washed second-stage leaching residue and washing water. The washing water was returned to the first-stage leaching reactor.
[0104] Lithium iron phosphate battery powder and a first-stage leachate were added to the reactor for neutralization. The mixture was stirred for 15 minutes to adjust the slurry temperature, and then stirred and reacted for another 1.5 hours at 80°C. After the reaction, the mixture was filtered through a vacuum filtration device to obtain a leachate with a pH of 0.7 and leachate residue 1. Leachate residue 1 was then subjected to a second-stage leaching process. The elemental contents of the leachate are shown in Table 1.
[0105] Copper removal by extraction The pH of the leachate to be treated was adjusted to 3 using 25% ammonia solution, and then extractant A (structural formula: M is polystyrene microspheres, i.e., resin 1) copper removal is performed by 4-column tandem extraction at an extraction flow rate of 2.0 Bv / h. After extraction saturation, the resin column is washed with dilute sulfuric acid solution. Aqueous phase extraction is completed, and copper removal raffinate is obtained.
[0106] Specifically, the washing can be carried out as follows: the saturated resin column is connected to the washing liquid pipeline, and a dilute sulfuric acid solution with a pH of 1.0 flows into the resin at a flow rate of 2.0 Bv / h, for a total of 5 Bv of washing liquid. After washing, the last effluent is taken to measure the content of elements such as iron, phosphorus, lithium, aluminum, titanium, and copper. After washing, the resin enters the back-extraction process. 5 Bv of 5 mol / L sulfuric acid back-extraction solution is taken and back-extracted at a flow rate of 0.2 Bv / h to obtain a copper-rich back-extraction solution.
[0107] Extraction to remove titanium and aluminum Extractant B after transformation was used (the alkaline solution used for neutralization and transformation was 5 mol / L ammonia water, and the structural formula of extractant B is as follows). M is polystyrene microspheres, i.e., resin 3) The copper-removed raffinate was subjected to 4-column tandem extraction to remove titanium and aluminum. The extraction flow rate was 1.2 Bv / H. After the extraction was saturated, the resin column was washed with pure water. The aqueous phase extraction was completed, and the titanium and aluminum-removed raffinate was obtained.
[0108] Specifically, the washing can be carried out as follows: the resin column saturated with extract is connected to the washing liquid pipeline, pure water flows into the resin at a flow rate of 1.5 Bv / h, and a total of 5 Bv of washing liquid is introduced. After washing, the last effluent is taken to measure the content of elements such as iron, phosphorus, lithium, aluminum, titanium, and copper. After washing, the resin enters the back-extraction process. 1 Bv of 2 mol / L sulfuric acid back-extraction solution (containing 32% hydrogen peroxide by mass, with the molar amount of hydrogen peroxide being twice that of titanium) is taken and back-extracted at 5 Bv / h for 1 hour. Then, the system is discharged at 1.5 Bv / h to obtain titanium-aluminum rich back-extraction solution.
[0109] The contents of major elements in the copper-free raffinate and the titanium-aluminum-free raffinate are shown in Table 1.
[0110] Table 1 The results showed that the copper content in the raffinate after copper removal was 0.002 g / L, while the aluminum and titanium contents were 0.52 g / L and 0.015 g / L, respectively, indicating good separation of copper from aluminum and titanium. After removing titanium and aluminum, the aluminum content in the raffinate was 0.002 g / L, and the titanium content was 0.0001 g / L.
[0111] Example 2 The leaching process was carried out as described in Example 1 to obtain the leachate to be treated.
[0112] Copper removal by extraction Extractant A was used after neutralization and transformation (the alkaline solution used for neutralization and transformation was 5 mol / L ammonia water, and the structural formula of extractant A was as follows). M is polystyrene microspheres, i.e., resin 2) It is subjected to 5-stage series extraction to remove copper. The extraction flow rate is 1.2 Bv / H. After the extraction is saturated, the resin column is washed with pure water. The aqueous phase extraction is completed, and the copper-removed raffinate is obtained.
[0113] Specifically, the washing can be carried out as follows: the extraction saturated resin column is connected to the washing liquid pipeline, pure water flows into the resin at a flow rate of 1.5 Bv / H, and a total of 5 Bv of washing liquid is introduced. After washing, the last effluent is taken to measure the content of elements such as iron, phosphorus, lithium, aluminum, titanium, and copper. After washing, the resin enters the back-extraction process. First, 0.5 Bv of 4 mol / L sulfuric acid back-extraction solution is taken and back-extracted at 5 Bv / h for 1 hour. Then, the system is discharged at 1.5 Bv / h to obtain copper-rich back-extraction solution.
[0114] Extraction to remove titanium and aluminum Extractant B after transformation (neutralization and transformation treatment is the same as in Example 1, and the structural formula of extractant B is as follows) M is polystyrene microspheres, i.e., resin 4). The copper-removed raffinate was subjected to 6-column tandem extraction to remove titanium and aluminum. The extraction flow rate was 1.2 Bv / h. After extraction saturation, the resin column was washed with pure water. The aqueous phase extraction was completed, and the titanium and aluminum-removed raffinate was obtained.
[0115] Specifically, the washing can be carried out as follows: the resin column saturated with extract is connected to the washing liquid pipeline, pure water flows into the resin at a flow rate of 1.5 Bv / h, and a total of 5 Bv of washing liquid is introduced. After washing, the last effluent is taken to measure the content of elements such as iron, phosphorus, lithium, aluminum, titanium, and copper. After washing, the resin enters the back-extraction process. 1 Bv of 2 mol / L sulfuric acid back-extraction solution (containing 32% hydrogen peroxide by mass concentration, with the molar amount of hydrogen peroxide being twice that of titanium) is taken and back-extracted at 5 Bv / h for 1 hour. Then, the system is discharged at 1.5 Bv / h to obtain titanium-aluminum rich back-extraction solution.
[0116] The contents of major elements in the copper-free raffinate and the titanium-aluminum-free raffinate are shown in Table 2.
[0117] Table 2 The results showed that the copper content in the raffinate after copper removal was 0.003 g / L, while the aluminum and titanium contents were 0.53 g / L and 0.045 g / L, respectively, indicating good separation of copper from titanium and aluminum. After removing titanium and aluminum, the aluminum content in the raffinate was 0.009 g / L, the titanium content was 0.0002 g / L, and the copper content was 0.002 g / L.
[0118] Example 3 The leaching process was carried out as described in Example 1 to obtain the leachate to be treated.
[0119] Copper removal by extraction The pH of the leachate to be treated was adjusted to 1.8 using 25% ammonia solution, and then extractant A (structural formula: M is polystyrene microspheres, i.e., resin 1) copper removal is performed by 4-column tandem extraction at an extraction flow rate of 1.2 Bv / h. After extraction saturation, the resin column is washed with dilute sulfuric acid. Aqueous phase extraction is completed, and copper removal raffinate is obtained.
[0120] Specifically, the washing can be carried out as follows: the saturated resin column is connected to the washing liquid pipeline, and a dilute sulfuric acid solution with a pH of 0.8 flows into the resin at a flow rate of 1.5 Bv / h, for a total of 5 Bv of washing liquid. After washing, the last effluent is taken to measure the content of elements such as iron, phosphorus, lithium, aluminum, titanium, and copper. After washing, the resin enters the back-extraction process. First, 0.5 Bv of 4 mol / L sulfuric acid back-extraction solution is taken and back-extracted at 5 Bv / h for 1 hour, and then discharged from the system at 1.5 Bv / h to obtain copper-rich back-extraction solution.
[0121] Extraction to remove titanium and aluminum Extractant B after transformation (neutralization and transformation treatment is the same as in Example 1, and the structural formula of extractant B is as follows) M is polystyrene microspheres, i.e., resin 5) The copper-removed raffinate was subjected to 4-column tandem extraction to remove titanium and aluminum. The extraction flow rate was 1.2 Bv / H. After the extraction was saturated, the resin column was washed with pure water. The aqueous phase extraction was completed, and the titanium and aluminum-removed raffinate was obtained.
[0122] Specifically, the washing can be carried out as follows: the resin column saturated with extract is connected to the washing liquid pipeline, pure water flows into the resin at a flow rate of 1.5 Bv / h, and a total of 5 Bv of washing liquid is introduced. After washing, the last effluent is taken to measure the content of elements such as iron, phosphorus, lithium, aluminum, titanium, and copper. After washing, the resin enters the back-extraction process. 1 Bv of 2 mol / L sulfuric acid back-extraction solution (containing 32% hydrogen peroxide by mass, with the molar amount of hydrogen peroxide being twice that of titanium) is taken and back-extracted at 5 Bv / h for 1 hour. Then, the system is discharged at 1.5 Bv / h to obtain titanium-aluminum rich back-extraction solution.
[0123] The contents of major elements in the copper-free raffinate and the titanium-aluminum-free raffinate are shown in Table 3.
[0124] Table 3 The results showed that the copper content in the raffinate after copper removal was 0.002 g / L, and the aluminum and titanium contents were 0.52 g / L and 0.03 g / L, respectively, indicating good separation of copper from titanium and aluminum. After removing titanium and aluminum, the aluminum content in the raffinate was 0.005 g / L, and the titanium content was 0.0001 g / L.
[0125] Comparative Example 1 Resin 6 was prepared according to the following synthetic route: Take 10 g (30 mmol, -NH2) primary amine polystyrene resin (from Samsung Resin, model SX382), 6.8 g (72 mmol) chloroacetic acid and 7.6 g (72 mmol) sodium carbonate into a 100 ml three-necked flask, add 50 mL of water, and heat at 80 °C for 12 hours under mechanical stirring to obtain resin 6.
[0126] The steps are the same as in Example 1, except that the extractant A has the following structural formula: M represents polystyrene microspheres, i.e., resin 6.
[0127] The results showed that the copper content in the raffinate after copper removal was 0.003 g / L, the titanium content was 0.0002 g / L, and the aluminum content was 0.02 g / L, indicating poor separation of copper from titanium and aluminum.
[0128] Comparative Example 2 Resin 7 was prepared according to the following synthetic route: Take 10 g (30 mmol, -NH2) primary amine polystyrene resin (from Samsung Resin, model SX382), 9.7 g (72 mmol) monochloropinazone and 7.6 g (72 mmol) sodium carbonate into a 100 ml three-necked flask, add 50 ml LDM, and heat at 80 °C for 12 hours under mechanical stirring to obtain resin 7.
[0129] The steps are the same as in Example 1, except that the extractant A has the following structural formula: M represents polystyrene microspheres, i.e., resin 7.
[0130] The results showed that the copper content in the raffinate after copper removal was 0.05 g / L, indicating poor copper removal efficiency.
[0131] The foregoing descriptions are merely exemplary embodiments or examples of the present invention and are not intended to limit the invention. Those skilled in the art will recognize that the present invention can be modified and varied in many ways. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principle of the present invention are included within the scope of the claims of this application.
Claims
1. A method for purifying and removing impurities from waste lithium iron phosphate powder, characterized in that, include: S1: Use an acidic solution to leach waste lithium iron phosphate powder to obtain a leachate containing iron, aluminum, titanium and copper; S2: Extract the leachate with extractant A to remove copper, and obtain copper-free raffinate A and copper-loaded extractant A; S3: Extract the copper-removed raffinate A with extractant B to remove titanium and aluminum, obtaining titanium and aluminum-removed raffinate B and titanium and aluminum-loaded extractant B. in, The extractant A comprises a chelating resin having the structure shown in Formula I: Equation I in: M is the resin matrix. R1 is selected from -(CH2) q -C(O)R5, R2 is selected from hydrogen or -(CH2). q -C(O)R5, R5 is selected from one or both C1-C. 10 An alkyl or alkenyl-substituted amino group, wherein the alkyl or alkenyl group is optionally substituted with a halogen; q is any integer from 1 to 4. The extractant B comprises a chelating resin having the structure shown in Formula II: Formula II in: M is the resin matrix. R3 is selected from -CH2-P(O)(R6)2. R4 is selected from hydrogen, -CH2-P(O)(R6)2, or -CHR8-(CH2). t -COR7, R6 is selected from -OH, -ONa, -OK, or optionally halogenated C1-C. 10 Alkoxy R7 is selected from hydroxyl groups, optionally halogenated C1-C. 10 Alkyl groups, or optionally one or two C1-C groups, are involved. 10 An alkyl or alkenyl-substituted amino group, wherein the alkyl or alkenyl group is optionally substituted with a halogen. R8 is selected from hydrogen, or optionally halogenated C1-C. 10 Alkyl groups or phenyl groups optionally substituted with C1-C4 alkyl groups or halogens, t is 0 or 1.
2. The method according to claim 1, characterized in that, The acid in the acidic solution is sulfuric acid.
3. The method according to claim 1, characterized in that, R5 is selected from amino groups that are optionally substituted with one or two C1-C4 alkyl groups; R7 is selected from hydroxyl, optionally halogenated C1-C4 alkoxy, or optionally substituted amino group with one or two C1-C6 alkyl groups; R8 is selected from hydrogen, optionally halogenated C1-C4 alkyl or phenyl.
4. The method according to any one of claims 1-3, characterized in that, In Formulas I and II, the resin matrix M is independently selected from polystyrene resin, copolymers of styrene and divinylbenzene, phenolic resin polymers, polyacrylic resin, and silicone resin.
5. The method according to any one of claims 1-3, characterized in that, In Equation I, q is 1 or 2.
6. The method according to any one of claims 1-3, characterized in that, The chelating resin having the structure of Formula I is selected from the following structures: 、 、 、 、 、 、 、 、 、 、 , M is independently selected from polystyrene resin, styrene-based copolymers with divinylbenzene.
7. The method according to any one of claims 1-3, characterized in that, The chelating resin having the structure of Formula II is selected from the following structures: 、 、 、 、 、 、 、 、 、 、 、 、 、 , M is independently selected from polystyrene resin, styrene-based copolymers with divinylbenzene.
8. The method according to any one of claims 1-3, characterized in that, The method also has one or more of the following features: 1) Before extraction, extractant A and extractant B are pretreated with alkaline solution for neutralization and transformation. 2) Before proceeding to step S2, adjust the pH of the leachate to 0.5-4.5.
Citation Information
Patent Citations
Method for synthesizing low-chloride polyphenylene sulfide resin
CN101665570A
Primary diamido chelating resin and preparation method thereof
CN103073667A