An iron-based high thermal conductivity medium entropy alloy for injection mold and a 3D printing method thereof

Through Fe-based high thermal conductivity medium entropy alloy and 3D printing process, combined with two-step tempering heat treatment, the thermal conductivity and cost problems of injection molds are solved, providing low-cost, rust-proof, high thermal conductivity injection mold materials, achieving high strength and Comprehensive performance with high thermal conductivity.

CN118497632BActive Publication Date: 2024-10-29SHANGHAI LAMO TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410956055.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-29
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Existing injection molds have bottlenecks in thermal conductivity and cost, especially when flow channels cannot be designed in complex structural locations. The strength and rust-proof performance of traditional materials are insufficient, and high thermal conductivity medium-entropy alloy materials are costly and difficult to pulverize.

Method used

Fe-based high thermal conductivity medium entropy alloy is used, containing 20%~30% Co element, 10%~15% Ni element, and 1%~5% Cu element. Through 3D printing process and two-step tempering heat treatment, it forms high thermal conductivity and high strength and toughness. material.

Benefits of technology

A low-cost, easy-to-produce, and rust-proof medium-entropy alloy material with high thermal conductivity and high thermal conductivity and strength has been achieved, which avoids material quenching deformation and reduces tissue stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118497632B_ABST
    Figure CN118497632B_ABST
Patent Text Reader

Abstract

The present invention discloses an iron-based medium-entropy alloy with high thermal conductivity for injection molds and a method for 3D printing thereof. The entropy alloy comprises 20% to 30% of Co element, 10% to 15% of Ni element, 1% to 5% of Cu element, and the balance of Fe element in terms of mass percentage. The 3D printing device adopts a strip scanning strategy to complete the molding on the substrate, and the substrate heating temperature is 100-180°C; after the molding is completed, the obtained workpiece is placed in a muffle furnace for heat treatment. The material of the present invention is an Fe-based medium-entropy alloy, and the Cu element is creatively designed to form a nano-scale Cu-rich phase, which improves the thermal conductivity of the material and greatly reduces the cost of the material. The present invention adopts a low-temperature tempering heat treatment process, retains the fine grain strengthening characteristics of 3D printing, and fully reduces the tissue stress, improves the toughness of the invented material, and ensures the toughness required by the mold. The present invention has low cost, high thermal conductivity, and good toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a low-cost Fe-based high thermal conductivity medium entropy alloy for injection molds and an additive manufacturing method thereof, belonging to the technical field of 3D printing. Background Art

[0002] In modern industrial production, molds are widely used in various fields, playing a key role in the manufacturing industry, and even directly determining the production efficiency, cost and quality of products. Molds are well-deserved mothers of industry. As one of the most important branches, injection molds can mass-produce plastic products with complex shapes. The reasonable design of molds is crucial to the quality of products, especially the temperature control system of molds, which has a particularly prominent impact on product quality.

[0003] As a new mold processing technology, 3D printing technology has been deeply applied in the field of injection molds because of its advantages in production cycle, design flexibility, customization and many other aspects. 3D printing technology, relying on strong design concepts, plays a more valuable role in the mold temperature control system than traditional manufacturing. In particular, the internal flow channel design of the mold that plays a cooling role plays a key role in product quality and production efficiency. At present, the cooling needs of injection molds are mainly achieved through three methods: conformal cooling water channels (molds manufactured by 3D printing), linear frame water channels (traditional mechanical processing methods or diffusion welding methods, cross-drilling methods to manufacture molds), and high thermal conductivity materials (beryllium copper, high thermal conductivity materials).

[0004] The mold structure is complex and changeable. There are often some characteristic structural positions that cannot be arranged with flow channels due to the constraints of strength properties, such as deep ribs and thin-walled positions. If the flow channels are not arranged at these positions, the strength of the structure will be affected. At present, there are three common treatment methods for positions where flow channels cannot be designed. The first is to extend the production cycle and wait for the special position to meet the cooling requirements before the next injection molding cycle. The second is to design beryllium copper or high thermal conductivity steel at this position. The mechanical strength and wear resistance of beryllium copper are both low, and beryllium copper is highly polluting during the processing process; in addition, the current traditional high thermal conductivity steel has poor rust resistance and is prone to rust during the production process, which is a great challenge to the stable production of molds. The third is to use 3D printing to print the mold with a high thermal conductivity medium entropy alloy to achieve cooling. For example, the patent CN 112301255 B mentioned in "A high thermal conductivity and high strength Co-Fe-Ni alloy for molds and its additive manufacturing method" has a higher thermal conductivity than traditional mold steel, but it is Co-based and has a high cost. For example, in the patent CN 116875868 A, "A high-strength, high-toughness, high-thermal-conductivity medium-entropy alloy and its preparation and application", the material described in the patent is also Co-based. In addition, due to the presence of Al elements in the design composition, the addition of Al will increase the difficulty of powder making, cause blockage, and significantly increase the cost. At the same time, in CN117483796A, "A two-phase high-entropy alloy based on 3D printing and its preparation method", the material described in the patent has good strength and plasticity but low thermal conductivity, high cost, and also contains a large amount of Al elements, which makes powder making difficult. Another example is CN116288049A, "A 3D printing high-strength and high-thermal-conductivity iron-based mold material and its preparation method and application", which describes a single matrix. The iron-based alloy is mainly composed of Fe elements, and its lattice structure is relatively simple, with less phonon scattering and higher thermal conductivity. However, the thermal conductivity of the iron-based alloy will decrease rapidly due to lattice defects and impurities. And as the temperature rises, the impurities and lattice defects in the iron-based alloy increase, and these factors will increase phonon scattering and further reduce thermal conductivity.

[0005] Therefore, the technical field urgently needs a low-cost, easy-to-produce, rust-proof, and 3D-printable high thermal conductivity medium-entropy alloy material for injection molds. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a type of low-cost, easy-to-produce, rust-proof, and 3D-printable high thermal conductivity medium-entropy alloy material for injection molds, so as to solve the bottleneck problem in the thermal conductivity application in the field of injection molds through the 3D printing production process.

[0007] In order to solve the above problems, the technical solution adopted by the present invention is: to provide an iron-based high thermal conductivity medium entropy alloy for injection molds, which includes 20%~30% Co element, 10%~15% Ni element, 1%~5% Cu element, and the balance Fe element in mass percentage.

[0008] The sum of the mass percentages of the above components is 100%.

[0009] The material of the present invention has high alloy strength and high thermal conductivity coefficient while being printable due to the ratio of Co, Ni and Cu elements.

[0010] In the present invention, Fe is used as the matrix, and Fe, Ni and Co elements form a medium entropy system, which greatly reduces the cost of alloy components. Cu element is creatively introduced, and Cu element exists as a nano-sized Cu-rich phase precipitation, which fully improves the thermal conductivity without damaging the toughness of the matrix.

[0011] The material of the present invention is combined with the 3D printing process to more easily obtain the comprehensive performance of high thermal conductivity and high strength and toughness. The present invention also provides a method for 3D printing of an iron-based high thermal conductivity medium entropy alloy for injection molds, characterized in that it includes the following steps:

[0012] Step 1): Weigh the metal powder of the corresponding elements according to the ratio, and use the strip scanning strategy through the 3D printing equipment to complete the molding on the substrate. The substrate heating temperature is 100-180℃;

[0013] Step 2): After the forming is completed, the workpiece is placed in a muffle furnace for heat treatment, and the heat treatment is protected by Ar atmosphere.

[0014] Preferably, in step 1), the molding power of the 3D printing equipment is 200-300W, the scanning speed is 600-800mm / s, and the layer thickness is 30-80μm.

[0015] Preferably, in step 2), the heat treatment is specifically as follows: the first step heat treatment temperature is 450-650°C, kept at temperature for 20-120 minutes, and air-cooled; the second step heat treatment temperature is 20-40°C lower than the first step heat treatment temperature, kept at temperature for 20-120 minutes, and air-cooled.

[0016] The material of the present invention is an Fe-based material, which has lower cost than other Co-based materials; the Cu element in the material of the present invention is precipitated in a Cu-rich phase, and has a high thermal conductivity; the material of the present invention is easy to form by 3D printing, adopts a two-step tempering heat treatment, has a simple process and fully reduces tissue stress.

[0017] After printing and heat treatment, the performance indicators of the material are as follows:

[0018] The hardness is 44~52HRC, the tensile strength is 1300~1500MPa, the yield strength is 1050~1400MPa, the Charpy V-notch impact energy is 10~45J, and the thermal conductivity is 50~70W / m•K.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. Low cost. The material of the present invention is an Fe-based medium-entropy alloy material. Compared with the Co-based medium-entropy alloy material, the cost of the alloy is low;

[0021] 2. Adding Cu element. The present invention innovatively adds Cu element, and Cu is precipitated in the form of nano-sized Cu-rich phase, which fully guarantees the creativity of the invented material without losing the toughness of the material;

[0022] 3. Two-step tempering heat treatment. The present invention adopts tempering heat treatment, which fully retains the fine grain strengthening characteristics of the 3D printing process, and chooses to reduce the heat treatment temperature of the second step by 20°C compared with the first step, which fully reduces the tissue stress and avoids the quenching deformation caused by the high temperature quenching heat treatment of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The microstructure of Fe: 57%, Co: 28%, Ni: 10%, Cu: 5% in Example 1 is a BCC matrix;

[0024] Figure 2 The precipitated phase distribution of Fe: 57%, Co: 28%, Ni: 10%, Cu: 5% in Example 1;

[0025] Figure 3 The precipitated phase composition and morphology of Fe: 58%, Co: 29%, Ni: 11%, and Cu: 2% in Example 4. DETAILED DESCRIPTION

[0026] In order to make the present invention more clearly understood, preferred embodiments are described in detail below with reference to the accompanying drawings.

[0027] Example 1

[0028] A low-cost Fe-based high thermal conductivity medium entropy alloy for injection molds and a 3D printing method thereof, wherein the powder composition is Fe: 57%, Co: 28%, Ni: 10%, Cu: 5%. The powder is prepared by vacuum melting gas atomization method: steel material is prepared according to the component ratio, the melting temperature is 1500-1600℃, the vacuum degree is 3-5Pa, and the atomization pressure is 3-5MPa.

[0029] The 3D printing method is

[0030] Step 1: Parts Printing

[0031] The powder was used to complete the molding on the substrate by adopting the strip scanning strategy, the substrate heating temperature was 100°C, the molding power was 260W, the scanning speed was 640mm / s, and the layer thickness was 40μm;

[0032] Step 2: Heat Treatment

[0033] After forming, the workpiece is subjected to two-step heat treatment.

[0034] The first step is heat treatment in a muffle furnace at 530°C for 30 min and air cooling.

[0035] The second step is 510℃, keep warm for 60min, and air cool. The heat treatment is protected by Ar atmosphere.

[0036] Example 2

[0037] A low-cost Fe-based high thermal conductivity medium entropy alloy for injection molds and a 3D printing method thereof, wherein the powder composition is Fe: 52%, Co: 29%, Ni: 15%, Cu: 4%. The powder is prepared by vacuum melting gas atomization method: steel material is prepared according to the component ratio, the melting temperature is 1500-1600℃, the vacuum degree is 3-5Pa, and the atomization pressure is 3-5MPa.

[0038] The 3D printing method is

[0039] Step 1: Parts Printing

[0040] Using the powder, a strip scanning strategy was adopted to complete the molding on the substrate, the substrate heating temperature was 150°C, the molding power was 280W, the scanning speed was 700mm / s, and the layer thickness was 50μm;

[0041] Step 2: Heat Treatment

[0042] After forming, the workpiece is subjected to two-step heat treatment.

[0043] The first step is heat treatment in a muffle furnace at 550°C for 30 min and air cooling.

[0044] The second step is 510℃, keep warm for 60min, and air cool. The heat treatment is protected by Ar atmosphere.

[0045] Example 3

[0046] A low-cost Fe-based high thermal conductivity medium entropy alloy for injection molds and a 3D printing method thereof, wherein the powder composition is Fe: 59%, Co: 29%, Ni: 11%, and Cu: 1%. The powder is prepared by vacuum melting gas atomization method: steel materials are prepared according to the component ratio, the melting temperature is 1500-1600℃, the vacuum degree is 3-5Pa, and the atomization pressure is 3-5MPa.

[0047] The 3D printing method is

[0048] Step 1: Parts Printing

[0049] The powder was used to complete the molding on the substrate by adopting a strip scanning strategy, the substrate heating temperature was 180°C, the molding power was 250W, the scanning speed was 650mm / s, and the layer thickness was 50μm;

[0050] Step 2: Heat Treatment

[0051] After forming, the workpiece is subjected to two-step heat treatment.

[0052] The first step is to place it in a muffle furnace for heat treatment at 560°C for 30 minutes and air cool it;

[0053] The second step is 540℃, keep warm for 60min, and air cool. The heat treatment is protected by Ar atmosphere.

[0054] Example 4

[0055] A low-cost Fe-based high thermal conductivity medium entropy alloy for injection molds and a 3D printing method thereof, wherein the powder composition is Fe: 58%, Co: 29%, Ni: 11%, Cu: 2%. The powder is prepared by vacuum melting gas atomization method: steel material is prepared according to the component ratio, the melting temperature is 1500-1600℃, the vacuum degree is 3-5Pa, and the atomization pressure is 3-5MPa.

[0056] The 3D printing method is

[0057] Step 1: Parts Printing

[0058] The powder was used to complete the molding on the substrate by adopting the strip scanning strategy, the substrate heating temperature was 180°C, the molding power was 230W, the scanning speed was 650mm / s, and the layer thickness was 50μm;

[0059] Step 2: Heat Treatment

[0060] After forming, the workpiece is subjected to two-step heat treatment.

[0061] The first step is heat treatment in a muffle furnace at 570°C for 30 min and air cooling.

[0062] The second step is 540℃, keep warm for 60min, and air cool. The heat treatment is protected by Ar atmosphere.

[0063] After testing, the performance of the molded workpiece at room temperature is shown in Table 1.

[0064] Table 1

[0065]

Claims

1. A method for 3D printing of an iron-based high thermal conductivity medium entropy alloy for injection molds, characterized in that: The iron-based high thermal conductivity medium entropy alloy for injection molds includes, by mass percentage, 20% to 30% of Co element, 10% to 15% of Ni element, 1% to 5% of Cu element, and the balance of Fe element; The 3D printing method comprises the following steps: Step 1): Weigh the metal powder of the corresponding elements according to the ratio, and use the strip scanning strategy through the 3D printing equipment to complete the molding on the substrate. The substrate heating temperature is 100-180℃; Step 2): After the forming is completed, the workpiece is placed in a muffle furnace for heat treatment, and the heat treatment is protected by Ar atmosphere.

2. The method for 3D printing of an iron-based high thermal conductivity medium entropy alloy for injection mold according to claim 1, characterized in that: In the step 1), the molding power of the 3D printing equipment is 200-300W, the scanning speed is 600-800mm / s, and the layer thickness is 30-80μm.

3. The method for 3D printing of an iron-based high thermal conductivity medium entropy alloy for injection mold according to claim 1, characterized in that: In the step 2), the heat treatment is specifically as follows: the first step heat treatment temperature is 450-650°C, kept at temperature for 20-120 minutes, and air-cooled; the second step heat treatment temperature is 20-40°C lower than the first step heat treatment temperature, kept at temperature for 20-120 minutes, and air-cooled.

Citation Information

Patent Citations

  • A high thermal conductivity and high strength Co-Fe-Ni alloy for molds and its additive manufacturing method.

    CN112301255B

  • 3D printing high-strength and high-thermal-conductivity iron-based mold material and preparation method and application thereof

    CN116288049A

  • Two-phase high-entropy alloy based on 3D printing and preparation method thereof

    CN117483796A

  • Soft magnetic film

    JP1991183743A