Photovoltaic cell and preparation method thereof, photovoltaic module
By using two-layer tunneling oxide layer and two-layer doped polysilicon layer structures in photovoltaic cells, combined with hot oxygen and then water oxygen deposition method and different temperature deposition processes, the H content of tunneling oxide layer and polysilicon layer is solved. The problem is that the conversion efficiency and passivation effect of photovoltaic cells are improved.
Patent Information
- Application Number
- CN202410980160.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-22
AI Technical Summary
In the existing photovoltaic cell manufacturing technology, the H content of the tunneled oxide layer and the polysilicon layer is easily reduced after high-temperature annealing, resulting in a reduction in the passivation effect, and the uniformity and cost problems of the passivation layer have not been effectively solved.
Using a passivation structure of two-layer tunneling oxide layer and two-layer doped polysilicon layer, the tunneling oxide layer is deposited by hot oxygen first and then water oxygen to increase the H content, and the doped polysilicon layer is deposited by different temperatures to form high and low barriers to improve carrier transmission efficiency.
The passivation effect of the passivation layer is significantly improved, the conversion efficiency of the solar cell is enhanced, the internal defect state density is reduced, and the process cost is relatively low.
Smart Images

Figure CN118507548B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of photovoltaic cell technology, and in particular to a photovoltaic cell and a preparation method thereof, and a photovoltaic module. Background Art
[0002] With the development of the solar photovoltaic market, people's demand for high-efficiency crystalline silicon cells is becoming more and more urgent. Due to the continuous development of photovoltaic technology, the manufacturing technology cost of photovoltaic cells is constantly decreasing, and the market competition is more intense. High-quality and low-cost photovoltaic cells are the main factors to improve competitiveness.
[0003] Topcon (Tunnel Oxide Passivated Contact) cell is a new type of passivated contact cell, which achieves passivation by coating an ultra-thin silicon oxide layer and doping polysilicon on the surface of the cell silicon substrate. IBC (Interdigitated Back Contact) cell and Topcon cell can be stacked to form TBC (Tunnel Back Contact) cell. TBC cell absorbs the tunnel oxide passivation contact technology of Topcon cell and the technology of preparing P and N regions arranged in interdigital shape on the back of IBC cell. Whether it is Topcon cell or TBC cell, how to form a passivation structure with better performance is the current research focus.
[0004] In addition, the current technologies for preparing the passivation layer mainly include plasma deposition, magnetron sputtering deposition and LPCVD (Low Pressure Chemical Vapor Deposition). The thickness of the tunneling oxide layer deposited by the plasma deposition method is not easy to accurately control, and amorphous silicon is prone to bubbling during subsequent annealing. The magnetron sputtering method has relatively poor uniformity, relatively high annealing temperature, and high cost. Therefore, LPCVD is the most commonly used deposition technology, but the LPCVD deposition method is subsequently subjected to high-temperature annealing, and the H content of the tunneling oxide layer and the polysilicon layer is greatly reduced, resulting in a decrease in its passivation effect. Therefore, there is a certain contradiction between annealing and hydrogen passivation, and how to further improve the passivation effect has become a difficulty. Summary of the invention
[0005] The purpose of the present application is to provide a photovoltaic cell, a preparation method thereof and a cell assembly. The photovoltaic cell provided in the present application has a good passivation structure, and its preparation method can effectively increase the H content in the tunneling oxide layer and the polysilicon layer, and effectively reduce the problem of increased internal defect state density caused by the subsequent high-temperature diffusion due to the reduction of H content.
[0006] The first aspect of the present application provides a photovoltaic cell, comprising: a silicon wafer and a passivation layer, wherein the passivation layer is sequentially provided with a first tunneling oxide layer, a first doped polysilicon layer, a second tunneling oxide layer and a second doped polysilicon layer on the first surface of the silicon wafer; wherein the first doped polysilicon layer and the second doped polysilicon layer have the same doping type, the doping concentration of the first doped polysilicon layer is less than the doping concentration of the second doped polysilicon layer, and when the doping type is N-type, the doping concentration of the first doped polysilicon layer is 1-2.5×10 20 / cm 3 The doping concentration of the second doped polysilicon layer is 3-5×10 20 / cm 3 When the doping type is P type, the doping concentration of the first doped polysilicon layer is 2-4×10 19 / cm 3 The doping concentration of the second doped polysilicon layer is 4-5×10 19 / cm 3 .
[0007] In an operative manner, the thickness of the first doped polysilicon layer is smaller than the thickness of the second doped polysilicon layer.
[0008] Preferably, the thickness of the first doped polysilicon layer is 10-80 nm.
[0009] Preferably, the thickness of the second doped polysilicon layer is 50-150 nm.
[0010] In an operative manner, the thickness of the first tunnel oxide layer is greater than the thickness of the second tunnel oxide layer.
[0011] In one practicable manner, the conductivity type of the silicon wafer is N-type.
[0012] In one practicable manner, the resistivity of the silicon wafer is 0.5-2Ω·cm.
[0013] A second aspect of the present application provides a method for preparing a photovoltaic cell, comprising the following steps:
[0014] Step 101: Select a silicon wafer and perform a texturing process on the silicon wafer;
[0015] Step 102: depositing a first tunneling oxide layer, a first amorphous silicon layer, a second tunneling oxide layer, and a second amorphous silicon layer in sequence on the surface of the silicon wafer;
[0016] Step 103: performing high temperature diffusion to form a passivation layer, wherein the formed passivation layer is the first tunneling oxide layer, the first doped polysilicon layer, the second tunneling oxide layer and the second doped polysilicon layer; the first doped polysilicon layer and the second doped polysilicon layer have the same doping type, and the doping concentration of the first doped polysilicon layer is less than the doping concentration of the second doped polysilicon layer; when the doping type is N-type, the doping concentration of the first doped polysilicon layer is 1-2.5×10 20 / cm 3 The doping concentration of the second doped polysilicon layer is 3-5×10 20 / cm 3 When the doping type is P type, the doping concentration of the first doped polysilicon layer is 2-4×10 19 / cm 3 The doping concentration of the second doped polysilicon layer is 4-5×10 19 / cm 3 .
[0017] In an practicable manner, in step 102, the first tunnel oxide layer and the second tunnel oxide layer are deposited by LPCVD;
[0018] The first tunneling oxide layer is deposited by first thermal oxidation and then water oxygen; wherein the ratio of the oxygen flow rate carried in the thermal oxidation process to that in the water oxygen process is 10:1-500:1; the ratio of the thermal oxidation to the water oxygen deposition time is 30:1-1:10; the thermal oxygen deposition temperature is 500-700°C; the water oxygen deposition temperature is 500-600°C;
[0019] The second tunneling oxide layer is prepared by a water-oxygen method; wherein the flow rate of oxygen and nitrogen in the water-oxygen is 1:50-1:2; the deposition temperature is 500-600° C., and the water-oxygen deposition time is 1 min-10 min.
[0020] Preferably, step 102: the deposition temperature of the first amorphous silicon layer is lower than the deposition temperature of the second amorphous silicon layer.
[0021] More preferably, the deposition temperature of the first amorphous silicon layer is 500-600°C; the deposition temperature of the second amorphous silicon layer is 500-700°C.
[0022] In an practicable manner, a gas flow rate when depositing the first amorphous silicon layer is greater than a gas flow rate when depositing the second amorphous silicon layer; and a deposition time of the first amorphous silicon layer is less than a deposition time of the second amorphous silicon layer.
[0023] The third aspect of the present application provides a photovoltaic assembly, comprising the photovoltaic cell of the first aspect of the present application or the photovoltaic cell prepared in the second aspect of the present application.
[0024] Compared with the prior art, this application:
[0025] (1) The passivation layer structure provided includes two tunneling oxide layers and two doped polysilicon layers, wherein the doping concentrations of the two doped polysilicon layers are different, and a tunneling oxide layer is provided in the two doped polysilicon layers, which can not only properly block the diffusion of doping elements into the lower tunneling oxide layer, but also form high and low potential barriers in the metallization areas of the lightly doped polysilicon layer and the heavily doped polysilicon layer, thereby improving the carrier transmission efficiency and making the solar cell conversion efficiency higher.
[0026] (2) The preparation method of the first tunnel oxide layer adopts thermal oxidation first and then water oxygen to supplement and increase the H content in the first tunnel oxide layer and the first amorphous silicon layer, which greatly reduces the problem of the increase of the internal defect state density caused by the subsequent high-temperature diffusion and the decrease of the H content, and can significantly improve the passivation effect of the passivation layer.
[0027] (3) The first doped layer and the second doped layer are deposited at different temperatures. The temperature of the first doped polysilicon layer is low, so that the H content in the first doped polysilicon layer is higher. In addition, the first doped polysilicon layer and the second doped polysilicon layer obtained by low temperature deposition are also more conducive to making the first tunneling oxide layer more uniform and flat. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0029] Figure 1 A schematic diagram showing an embodiment of a passivation layer structure of a photovoltaic cell of the present application.
[0030] Figure 2 A schematic diagram showing the passivation layer structure of a prior art photovoltaic cell.
[0031] Figure 3 A schematic flow chart of an embodiment of a method for preparing a photovoltaic cell of the present application is shown.
[0032] Reference numerals:
[0033] 1-silicon wafer; 1'-silicon wafer; 2-first tunneling oxide layer; 2'-tunneling oxide layer; 3-first doped polysilicon layer; 4-second tunneling oxide layer; 5-second doped polysilicon layer; 5'-doped polysilicon layer. DETAILED DESCRIPTION
[0034] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.
[0035] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, "multiple" means two or more, unless otherwise clearly and specifically defined. "Several" means one or more, unless otherwise clearly and specifically defined.
[0036] like Figure 2 As shown, in the prior art, the silicon wafer 1' includes a passivation layer, and the structure of the passivation layer is mainly composed of a tunneling oxide layer 2' and a doped polysilicon layer 5'. Since the doping elements in the doped polysilicon layer 5' will diffuse into the tunneling oxide layer 2', the carrier transmission effect is reduced, so that the improvement of the conversion efficiency of the solar cell is limited.
[0037] To this end, the first aspect of the present application provides a photovoltaic cell, such as Figure 1 As shown, the photovoltaic cell includes: a silicon wafer 1 and a passivation layer; the passivation layer is a first tunneling oxide layer 2, a first doped polysilicon layer 3, a second tunneling oxide layer 4 and a second doped polysilicon layer 5 on a first surface of the silicon wafer 1.
[0038] The silicon wafer 1 can be an N-type single crystal silicon wafer or a P-type single crystal silicon wafer; in the process of preparing the silicon wafer into a battery, it will be divided into the front and the back; the first surface of the silicon wafer can be the front of the subsequent battery cell or the back of the subsequent battery cell, which is related to the photovoltaic cell structure prepared subsequently and the doping type of its passivation layer; for example, when preparing a Topcon battery, an N-type single crystal silicon wafer is used. If an N-type doped polycrystalline silicon layer is used, the passivation layer is arranged on the back. At this time, the first surface of the silicon wafer of the present application is the back of the subsequent battery cell; when preparing a Topcon battery, an N-type single crystal silicon wafer is used. If a P-type doped polycrystalline silicon layer is used, the passivation layer is arranged on the front. At this time, the first surface of the silicon wafer of the present application is the front of the subsequent battery cell; when preparing a TBC battery, whether it is an N-type single crystal silicon wafer or a P-type polycrystalline silicon wafer, whether it is an N-type or P-type doped polycrystalline silicon layer, the passivation layer is arranged on the back. The first surface of the silicon wafer of the present application is the back of the subsequent battery cell.
[0039] The first doped polysilicon layer and the second doped polysilicon layer have the same doping type, and the doping concentration of the first doped polysilicon layer is less than the doping concentration of the second doped polysilicon layer; since the second tunneling oxide layer can prevent the diffusion of the doping elements in the first doped polysilicon layer, it is necessary to reduce the concentration in the first doped polysilicon layer to avoid excessive expansion of the first doped polysilicon layer into the first tunneling oxide layer.
[0040] The doping type of the first doped polysilicon layer and the second doped polysilicon layer can be N-type or P-type. When the doping type is N-type, the doping concentration of the first doped polysilicon layer is 1-2.5×10 20 / cm 3 , for example, it can be 1×10 20 / cm 3 , 1.1×10 20 / cm 3 , 1.2×10 20 / cm 3 , 1.3×10 20 / cm 3 , 1.4×10 20 / cm 3 , 1.5×10 20 / cm 3 , 1.6×10 20 / cm 3 , 1.7×10 20 / cm 3 , 1.8×10 20 / cm 3 , 1.9×10 20 / cm 3 , 2.0×10 20 / cm 3 , 2.1×10 20 / cm 3 , 2.2×10 20 / cm 3 , 2.3×10 20 / cm 3 , 2.4×10 20 / cm 3 or 2.5 × 10 20 / cm 3 And the range value of any two points. The doping concentration of the second doped polysilicon layer is 3-5×10 20 / cm 3 , for example, it can be 3×10 20 / cm 3 , 3.1×10 20 / cm 3 , 3.2×10 20 / cm 3, 3.3×10 20 / cm 3 , 3.4×10 20 / cm 3 , 3.5×10 20 / cm 3 , 3.6×10 20 / cm 3 , 3.7×10 20 / cm 3 , 3.8×10 20 / cm 3 , 3.9×10 20 / cm 3 4.0×10 20 / cm 3 4.1×10 20 / cm 3 4.2×10 20 / cm 3 , 4.3×10 20 / cm 3 , 4.4×10 20 / cm 3 , 4.5×10 20 / cm 3 , 4.6×10 20 / cm 3 , 4.7×10 20 / cm 3 , 4.8×10 20 / cm 3 , 4.9×10 20 / cm 3 or 5.0×10 20 / cm 3 When the doping type is P-type, the doping concentration of the first doped polysilicon layer is 2-4×10 19 / cm 3 , for example, it can be 2.0×10 19 / cm 3 , 2.1×10 19 / cm 3 , 2.2×10 19 / cm 3 , 2.3×10 19 / cm 3 , 2.4×10 19 / cm 3 , 2.5×10 19 / cm 3 , 3×10 19 / cm 3 , 3.1×10 19 / cm3 , 3.2×10 19 / cm 3 , 3.3×10 19 / cm 3 , 3.4×10 19 / cm 3 , 3.5×10 19 / cm 3 , 3.6×10 19 / cm 3 , 3.7×10 19 / cm 3 , 3.8×10 19 / cm 3 , 3.9×10 19 / cm 3 or 4.0×10 19 / cm 3 And the range value of any two points. The doping concentration of the second doped polysilicon layer is 4-5×10 19 / cm 3 , for example, it can be 4.0×10 19 / cm 3 4.1×10 19 / cm 3 4.2×10 19 / cm 3 , 4.3×10 19 / cm 3 , 4.4×10 19 / cm 3 , 4.5×10 19 / cm 3 , 4.6×10 19 / cm 3 , 4.7×10 19 cm 3 , 4.8×10 19 / cm 3 , 4.9×10 19 / cm 3 or 5.0×10 19 / cm 3 And the range value of any two points. The concentration of the first doped polysilicon layer and the second doped polysilicon layer affects the effect of the tunneling layer and the electrical properties of the cell. If the concentration of the first doped polysilicon layer and the second doped polysilicon layer is too low, the square resistance is too high during the preparation of the cell, resulting in poor FF of the cell prepared later, affecting the cell efficiency of the cell. If the concentration of the first doped polysilicon layer and the second doped polysilicon layer is too high, the doping elements in the first doped polysilicon layer or the second doped polysilicon layer will cause the doping elements to expand severely in the first tunneling oxide layer, affecting the tunneling effect.
[0041] By preparing a passivation layer structure with two tunneling oxide layers and two doped polysilicon layers, the doping concentrations of the two doped polysilicon layers are different, and a tunneling oxide layer is set in the two doped polysilicon layers, which can not only properly block the diffusion of doping elements to the lower tunneling oxide layer, but also form high and low potential barriers in the metallization areas of the lightly doped polysilicon layer and the heavily doped polysilicon layer, thereby improving the carrier transmission efficiency and making the solar cell conversion efficiency higher.
[0042] In an illustrative embodiment, the thickness of the first doped polysilicon layer is smaller than the thickness of the second doped polysilicon layer.
[0043] In some specific embodiments, the thickness of the first doped polysilicon layer is 10-80 nm; for example, it can be 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 22 nm, 24 nm, 25 nm, 26 nm, 28 nm, 29 nm, 30 nm, 32 nm, 35 nm, 40 nm, 45 nm, 50 nm, 53 nm, 55 nm, 57 nm, 60 nm, 62 nm, 64 nm, 65 nm, 66 nm, 68 nm, 69 nm, 70 nm, 72 nm, 75 nm, 78 nm or 80 nm, and a range of values between any two points.
[0044] In some specific embodiments, the thickness of the second doped polysilicon layer is 50-150 nm, for example, it can be 50 nm, 53 nm, 55 nm, 57 nm, 60 nm, 62 nm, 64 nm, 65 nm, 66 nm, 68 nm, 69 nm, 70 nm, 72 nm, 75 nm, 78 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, 105 nm, 110 nm, 115 nm, 120 nm, 125 nm, 130 nm, 135 nm, 140 nm, 145 nm or 150 nm and a range of values between any two points.
[0045] In an illustrative embodiment, the thickness of the first tunnel oxide layer is greater than the thickness of the second tunnel oxide layer.
[0046] In some specific embodiments, the ratio of the thickness of the first tunnel oxide layer to the thickness of the second tunnel oxide layer is 1:2-1:10; for example, it can be 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10 and a range value between any two points.
[0047] In a more specific embodiment, the thickness of the first tunnel oxide layer is 1.5-2 nm; for example, it can be 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm, 1.9 nm or 2 nm and the range value between any two points; the thickness of the second tunnel oxide layer is 1-1.5 nm; for example, it can be 1 nm, 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm or 1.5 nm and the range value between any two points.
[0048] In some specific embodiments, the resistivity of the silicon wafer is 0.5-2Ω·cm; for example, it may be 0.5Ω·cm, 0.6Ω·cm, 0.8Ω·cm, 1.0Ω·cm, 1.5Ω·cm or 2Ω·cm and a range of values between any two points.
[0049] In some specific embodiments, the doping type of the first doped polysilicon layer and the second doped polysilicon layer is P-type; preferably, the doping element of the first doped polysilicon layer and the second doped polysilicon layer is both boron.
[0050] In some specific embodiments, the doping type of the first doped polysilicon layer and the second doped polysilicon layer is N-type; preferably, the doping elements of the first doped polysilicon layer and the second doped polysilicon layer are both phosphorus.
[0051] In some specific embodiments, the photovoltaic cell is a Topcon cell or a TBC cell.
[0052] The second aspect of the present application provides a method for preparing a photovoltaic cell, such as Figure 3 As shown, the following steps are included:
[0053] Step 101: Select a single crystal silicon wafer and perform a texturing process on the silicon wafer;
[0054] In this step, the monocrystalline silicon wafer, as the raw material for preparing the solar cell, can be an N-type monocrystalline silicon wafer or a P-type monocrystalline silicon wafer; in the process of preparing the silicon wafer into the solar cell, the two oppositely arranged surfaces of the silicon wafer will be divided into the front side and the back side according to the subsequent light receiving effect; the front side is the side that mainly faces the sunlight after being prepared into a photovoltaic module; the back side is the side that is relatively away from the sunlight after being prepared into a photovoltaic module. Structurally, the front side is generally the side that is close to the glass in the photovoltaic module after being prepared into a photovoltaic module, and is the side that mainly absorbs sunlight; the back side is the side that is away from the glass in the photovoltaic module.
[0055] In this step, the front side of the silicon wafer is subjected to a texturing treatment to obtain a pyramid-structured texturing surface on the surface of the silicon wafer.
[0056] In one practicable manner, after the silicon wafer is textured, the first surface of the silicon wafer is subjected to alkali polishing to form a polished surface on the first surface of the silicon wafer, thereby being more conducive to the preparation of the passivation layer. Alkali texture treatment and alkali polishing are conventional techniques for preparing solar cells and will not be described in detail here.
[0057] Alkali polishing is mainly to form a polished surface on the surface where the passivation layer is located, which is more conducive to the setting of the passivation layer. The first surface of the present application is provided with a passivation layer. The first surface can be the front side of the silicon wafer or the surface of the silicon wafer, which is related to the structure of the photovoltaic cell prepared subsequently and the doping type of its passivation layer.
[0058] In a specific embodiment, when preparing a Topcon cell, an N-type monocrystalline silicon wafer and an N-type doped polycrystalline silicon layer are used, the first surface of the silicon wafer is the back side, and the back side of the silicon wafer is alkaline polished;
[0059] In a specific embodiment, when preparing a Topcon cell, an N-type monocrystalline silicon wafer and a P-type doped polycrystalline silicon layer are used, the first surface of the silicon wafer is the front side, and the front side of the silicon wafer is alkaline polished;
[0060] In a specific embodiment, when preparing a TBC cell, the first surface of the silicon wafer is the back surface, and the back surface of the silicon wafer is alkaline polished.
[0061] Step 102: depositing a first tunneling oxide layer, a first amorphous silicon layer, a second tunneling oxide layer, and a second amorphous silicon layer in sequence on the surface of the silicon wafer;
[0062] In this step, a passivation layer is prepared on the surface of the silicon wafer. First, a first tunneling oxide layer, a first amorphous silicon layer, a second tunneling oxide layer and a second amorphous silicon layer are sequentially deposited on the surface of the silicon wafer; wherein the first tunneling oxide layer and the second tunneling oxide layer can be prepared by LPCVD deposition.
[0063] Here, the surface of the silicon wafer refers to the first surface of the silicon wafer and the second surface of the silicon wafer; as before, the two oppositely disposed surfaces of the silicon wafer will be divided into the front side and the back side according to the subsequent light receiving effect; and due to the structure of the photovoltaic cell prepared subsequently and the doping type of its passivation layer; the first surface of the silicon wafer can be the front side of the silicon wafer or the back side of the silicon wafer; the second surface of the silicon wafer is the other side opposite to the first surface of the silicon wafer; for example, when the first surface of the silicon wafer is the front side of the silicon wafer, the second surface of the silicon wafer is the back side of the silicon wafer; when the first surface of the silicon wafer is the back side of the silicon wafer, the second surface of the silicon wafer is the front side of the silicon wafer.
[0064] In an practicable manner, the first tunnel oxide layer is deposited by first thermal oxidation and then water oxygenation. The combination of thermal oxidation and water oxygenation can replenish and increase the hydrogen content in the tunnel oxide layer and the first amorphous silicon layer, significantly improving the passivation effect of the passivation layer.
[0065] The hot oxygen referred to in this application refers to dry oxygen oxidation, that is, it is carried out in a high temperature, dry and pure oxygen atmosphere, so that the thin layer of silicon on the surface of the silicon wafer is converted into silicon dioxide; the water oxygen referred to in this application refers to the conversion of the thin layer of silicon on the surface of the silicon wafer into silicon dioxide in a high temperature, pure oxygen and pure water vapor mixed atmosphere; wherein, in the water oxygen process, the water vapor content is 100-1000sccm; the oxygen content is 100sccm~1000sccm. Specifically, the ratio of the flow rate of oxygen carried in the thermal oxygen process to the flow rate of oxygen carried in the water oxygen process is 10:1~500:1; for example, it can be 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, 30:1, 40:1, 50:1, 60:1, 70:1, 80:1, 90:1, 100:1, 110:1, 120:1, 130:1, 150:1, 170:1, 180:1, 200:1, 250:1, 300:1, 350:1, 400:1, 450:1 or 500:1 and the range value between any two points.
[0066] Preferably, the flow rate of oxygen carried in the thermal oxygen process is 10000sccm to 50000sccm; for example, it can be 10000sccm, 20000sccm, 30000sccm, 40000sccm or 50000sccm and the range value between any two points; the flow rate of oxygen carried in the water oxygen process is 100sccm to 1000sccm; for example, it can be 100sccm, 200sccm, 300sccm, 400sccm, 500sccm, 600sccm, 700sccm, 800sccm, 900sccm or 1000sccm and the range value between any two points.
[0067] Specifically, the ratio of the time of thermal oxygen to water oxygen deposition is 30:1~1:10; for example, it can be 30:1, 20:1, 10:1, 1:1, 1:2, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10 and a range of values between any two points.
[0068] Preferably, the time of thermal oxygen deposition is 1 min to 30 min; for example, it can be 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min or 30 min. The time of water oxygen deposition is 1 min to 10 min; for example, it can be 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min.
[0069] Specifically, the deposition temperature of thermal oxygen is 500-700°C; for example, it can be 500°C, 550°C, 600°C, 650°C or 700°C; the deposition temperature of water oxygen is 500-600°C; for example, it can be 500°C, 550°C or 600°C.
[0070] In an practicable manner, the second tunneling oxide layer is prepared by a water-oxygen method;
[0071] Specifically, the flow ratio of oxygen to nitrogen in water oxygen is 1:50 to 1:2; for example, it can be 1:50, 1:40, 1:30, 1:20, 1:10, 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, 1:3 or 1:2;
[0072] Preferably, the flow rate of oxygen carried in water oxygen is 100~1000sccm, for example, it can be 500sccm, 600sccm, 700sccm, 800sccm, 900sccm or 1000sccm and the range value between any two points; the flow rate of nitrogen is 1000~5000sccm; for example, it can be 1000sccm, 2000sccm, 3000sccm, 4000sccm or 5000sccm and the range value between any two points.
[0073] Specifically, the deposition temperature of water oxygen is 500-600° C.; for example, it can be 500° C., 550° C. or 600° C., or a range value between any two points.
[0074] Specifically, the time for water oxygen deposition is 1 min to 10 min; for example, it can be 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, and a range value between any two points.
[0075] In an operative manner, the first amorphous silicon layer and the second amorphous silicon layer are deposited by LPCVD; the deposition temperature of the first amorphous silicon layer is lower than the deposition temperature of the second amorphous silicon layer. By controlling the deposition temperatures of the first amorphous silicon layer and the second amorphous silicon layer, the H content in the first amorphous silicon layer can be controlled. In addition, low-temperature deposition also makes the subsequent doped polysilicon layer more uniform and flat when tunneling through the oxide layer.
[0076] In a specific embodiment, the deposition temperature of the first amorphous silicon layer is 500-600° C., for example, it can be 500° C., 550° C., or 600° C., or a range of any two points. The deposition temperature of the second amorphous silicon layer is 500-700° C., for example, it can be 500° C., 550° C., 600° C., 650° C., or 700° C., or a range of any two points.
[0077] In an practicable manner, the gas flow rate when depositing the first amorphous silicon layer is greater than the gas flow rate when depositing the second amorphous silicon layer; the deposition time of the first amorphous silicon layer is less than the deposition time of the second amorphous silicon layer. By controlling the gas flow rate and deposition time of the first amorphous silicon layer and the second amorphous silicon layer, doped polysilicon layers of different thicknesses can be controlled.
[0078] Specifically, the first amorphous silicon layer is deposited at 1000 sccm to 2000 sccm, for example, 1000 sccm, 1100 sccm, 1200 sccm, 1300 sccm, 1400 sccm, 1500 sccm, 1600 sccm, 1700 sccm, 1800 sccm, 1900 sccm or 2000 sccm and a range value between any two points. The gas flow rate for depositing the second amorphous silicon layer is 1000 sccm to 2000 sccm, for example, 1000 sccm, 1100 sccm, 1200 sccm, 1300 sccm, 1400 sccm, 1500 sccm, 1600 sccm, 1700 sccm, 1800 sccm, 1900 sccm or 2000 sccm and a range value between any two points. The deposition time of the first amorphous silicon layer is 1 min to 15 min, for example, it can be 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min or 15 min, and the range between any two points. The deposition time of the second amorphous silicon layer is 10 min to 30 min, for example, it can be 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min or 30 min, and the range between any two points.
[0079] Specifically, the gas for depositing the first amorphous silicon layer and the gas for depositing the second amorphous silicon layer is SiH 4 .
[0080] Step 103: Perform high temperature diffusion to form a passivation layer, wherein the formed passivation layer is a first tunneling oxide layer, a first doped polysilicon layer, a second tunneling oxide layer and a second doped polysilicon layer; the first doped polysilicon layer and the second doped polysilicon layer have the same doping type, and the doping concentration of the first doped polysilicon layer is less than the doping concentration of the second doped polysilicon layer; when the doping type is N-type, the doping concentration of the first doped polysilicon layer is 1-2.5×10 20 / cm 3 The doping concentration of the second doped polysilicon layer is 3-5×10 20 / cm 3 When the doping type is P type, the doping concentration of the first doped polysilicon layer is 2-4×10 19 / cm 3 The doping concentration of the second doped polysilicon layer is 4-5×10 19 / cm 3 .
[0081] In this step, the first tunneling oxide layer, the first amorphous silicon layer, the second tunneling oxide layer and the second amorphous silicon layer are formed into a first tunneling oxide layer, a first doped polysilicon layer, a second tunneling oxide layer and a second doped polysilicon layer through high temperature diffusion.
[0082] Specifically, the high temperature diffusion can be processed by diffusion using BCL3 or POCL3 gas.
[0083] In one practicable manner, the method for preparing a Topcon photovoltaic cell further comprises:
[0084] Step 101-1: boron-doping and BSG (borosilicate glass) removal are performed on the second surface of the silicon wafer to obtain P+ polysilicon; this step is performed after step 101, after the silicon wafer is subjected to texturing treatment, if there is alkali polishing, before alkali polishing and after texturing, the second surface of the silicon wafer is subjected to boron-doping and BSG removal to obtain P+ polysilicon; the preparation of P+ polysilicon is a prior art and will not be described in detail in this application.
[0085] In one practicable manner, the method for preparing a Topcon photovoltaic cell further comprises:
[0086] Step 104: cleaning the plated and doped polysilicon layer and the tunnel oxide layer on the second surface of the silicon wafer; after cleaning, depositing an aluminum oxide layer and a first anti-reflection film layer;
[0087] Subsequently, a second anti-reflection film layer is deposited on the first surface of the silicon wafer;
[0088] Finally, electrodes are printed on the first surface and the second surface of the silicon wafer; and metal electrodes are obtained through sintering and laser.
[0089] In this step, since the passivation layer structure formed in step 103 exists on both the first surface and the second surface of the silicon wafer, the passivation layer on the second surface where the passivation layer is not needed is removed, and the removal can be performed by cleaning, such as RCA. After the cleaning is completed, an aluminum oxide layer and a first anti-reflection film layer are deposited on the second surface of the silicon wafer;
[0090] Subsequently, a second anti-reflection film layer is deposited on the first surface of the silicon wafer, that is, on the passivation layer.
[0091] Finally, electrodes are formed on the first surface and the second surface of the silicon wafer to complete the preparation of the photovoltaic cell.
[0092] The preparation of the aluminum oxide passivation layer, the first anti-reflection film layer, the second anti-reflection film layer and the electrode belongs to the common technology in this field and will not be described in detail here.
[0093] The third aspect of the present application provides a photovoltaic module, comprising the photovoltaic cell of the first aspect of the present application or the photovoltaic cell prepared by the third aspect of the present application.
[0094] The following describes in detail the preparation method of the photovoltaic cell disclosed in the first aspect and the photovoltaic cell disclosed in the second aspect of the present application with several specific embodiments. It is worth noting that the following description is only for illustrative purposes and is not a specific limitation of the invention.
[0095] Example 1
[0096] The photovoltaic cell is a Topcon cell, and the structure of the photovoltaic cell includes a silicon wafer 1, which is an N-type single-crystal silicon wafer. A first tunneling oxide layer 2, a first doped polysilicon layer 3, a second tunneling oxide layer 4, a second doped polysilicon layer 5, a second anti-reflection film layer and a back electrode are sequentially arranged on the first surface of the silicon wafer 1; a P+ emitter layer, an aluminum oxide passivation layer, a first anti-reflection film layer and a front electrode are sequentially arranged on the second surface of the silicon wafer.
[0097] The thickness of the first tunnel oxide layer 2 is 1.5 nm, the thickness of the first doped polysilicon layer 3 is 40 nm, the thickness of the second tunnel oxide layer 4 is 1 nm, and the thickness of the second doped polysilicon layer 5 is 120 nm. P-type doping is selected, and the doping concentration of the first doped polysilicon layer is 2.12×10 19 / cm 3 The doping concentration of the second doped polysilicon layer is 4.65×10 19 / cm 3 .
[0098] The Sinton tester is used to test the minority carrier lifetime of photovoltaic cells; the battery efficiency tester is used to test the electrical performance of photovoltaic cells.
[0099] Example 2
[0100] The difference between Example 2 and Example 1 is that the photovoltaic cell is a TBC cell.
[0101] The structure of the photovoltaic cell includes a silicon wafer 1, which is an N-type single crystal silicon wafer. The first semiconductor layer, the second semiconductor layer and the back electrode are alternately arranged on the first surface of the silicon wafer. The first semiconductor layer includes a first passivation layer; and a second anti-reflection layer; the second semiconductor layer includes a second passivation layer and a third anti-reflection layer arranged outward in sequence. The aluminum oxide passivation layer, the first anti-reflection film layer and the front electrode are arranged in sequence on the second surface of the silicon wafer;
[0102] The first passivation layer and the second passivation layer are both prepared by a first tunneling oxide layer 2, a first doped polysilicon layer 3, a second tunneling oxide layer 4 and a second doped polysilicon layer 5;
[0103] Among them, the thickness of the first tunneling oxide layer 2 is 1.5 nm, the thickness of the first doped polysilicon layer 3 is 40 nm, the thickness of the second tunneling oxide layer 4 is 1 nm, and the thickness of the second doped polysilicon layer 5 is 120 nm;
[0104] The first doped polysilicon layer 3 and the second doped polysilicon layer 5 of the first passivation layer are N-type; the doping concentration of the first doped polysilicon layer is 2.5×10 20 / cm 3 The doping concentration of the second doped polysilicon layer is 3.5×10 20 cm 3 ;
[0105] The first doped polysilicon layer 3 and the second doped polysilicon layer 5 of the first passivation layer are P-type; the doping concentration of the first doped polysilicon layer is 2.12×10 19 / cm 3 The doping concentration of the second doped polysilicon layer is 4.65×10 19 / cm 3 .
[0106] Comparative Example 1
[0107] Comparative Example 1 Compared with Example 1, a tunneling oxide layer and a doped polysilicon layer are sequentially provided on the first surface of the silicon wafer 1. The thickness of the tunneling oxide layer is 1.5 nm, the thickness of the doped polysilicon layer is 160 nm, the doping element is P-type, and the doping concentration is 4.45×10 19 / cm3.
[0108] Comparative Example 2
[0109] The difference between Comparative Example 2 and Example 2 is that,
[0110] The first passivation layer and the second passivation layer are both prepared from a tunneling oxide layer and a doped polysilicon layer;
[0111] Among them, the thickness of the tunnel oxide layer is 1.5nm, and the thickness of the doped polysilicon layer is 160nm;
[0112] The doped polysilicon layer of the first passivation layer is N-type with a doping concentration of 3.5×10 20 cm 3 ;
[0113] The doping element of the second passivation layer is P-type, and the doping concentration is 4.45×10 19 / cm3.
[0114] Comparative Example 3
[0115] The difference between Comparative Example 3 and Example 1 is that the doping concentration of the first doped polysilicon layer and the doping concentration of the second doped polysilicon layer are equal, which is 4.65×1019 / cm3.
[0116] Table 1 below shows the test data of Examples 1-2 and Comparative Examples 1-3, where minority carrier lifetime is minority carrier lifetime, Jo is saturation current, Voc is open circuit voltage, and FF is fill factor. As can be seen from the table, (1) compared with Comparative Example 1, the minority carrier lifetime value, Voc and FF of Example 1 increase, Jo decreases, and the electrical performance is significantly improved. (2) compared with Comparative Example 2, the minority carrier lifetime value, Voc and FF of Example 2 increase, Jo decreases, and the electrical performance is significantly improved. (3) compared with Comparative Example 1 and Example 1, since the doping concentration of the first doped polysilicon layer and the doping concentration of the second doped polysilicon layer used in Comparative Example 3 are equal, high and low potential barriers cannot be formed, and its minority carrier lifetime value, Voc and FF are all reduced compared with Comparative Example 1, and Jo also increases, which has a counter-effect.
[0117] Table 1 Test data of Examples 1-2 and Comparative Examples 1-3
[0118]
[0119] Example 3
[0120] Preparation of Topcon cells;
[0121] Step 101: Select an N-type single crystal silicon wafer, the resistivity of the silicon wafer is 0.5-2Ω·cm, the size of the silicon wafer is 182×182mm, and the thickness is ~130μm, and perform alkali texturing treatment on the second surface of the silicon wafer;
[0122] Then, boron is diffused by thermal diffusion to form a P+ emitter layer, and then the side junction is removed cleanly, and the BSG layer (borosilicate glass layer) is retained on the second surface, and the back side is alkaline polished;
[0123] Step 102: depositing a first tunneling oxide layer, a first amorphous silicon layer, a second tunneling oxide layer, and a second amorphous silicon layer in sequence on a first surface of the silicon wafer;
[0124] First, the first tunnel oxide layer is deposited, first using a thermal oxygen method, with a gas flow rate of 30000sccm, a temperature of 580°C, a pressure of 600mtorr, and a process time of 2min, then using a water oxygen method, with a water oxygen gas flow rate of 220sccm, a diluted nitrogen gas of 1800sccm, a temperature of 580°C, a pressure of 600mtorr, and a process time of 2min, then without passing gas, at a temperature of 580°C, and a process time of 10min;
[0125] Then the first amorphous silicon layer was deposited, with a SiH4 flow rate of 1600 sccm, a temperature of 580°C, a pressure of 180 mtorr, and a process time of 7 min;
[0126] Then, the second tunnel oxide layer was deposited by water-oxygen method, with a water-oxygen gas flow rate of 200 sccm, a diluted nitrogen gas of 2000 sccm, a temperature of 580°C, a pressure of 600 mtorr, and a process time of 3 minutes. Then, no gas was passed, the existing temperature of 580°C was maintained, and the process time was 8 minutes.
[0127] Finally, the second amorphous silicon layer was deposited by first increasing the temperature to 610°C, then introducing SiH4 at a flow rate of 1300 sccm, a pressure of 180 mtorr, and a process time of 25 min.
[0128] Step 103: performing high temperature diffusion to form a passivation layer;
[0129] The amorphous silicon layer is doped with phosphorus at high temperature, and phosphorus oxychloride is selected as the doping source. The doping source flow rate of the source step is 1850sccm, the pressure is 150bar, the temperature is 800℃, and the time is 650 seconds. The pressure of the annealing step is 300bar, the temperature is 880℃, and the process time is 1300 seconds.
[0130] Subsequently, the PSG layer, N+ polysilicon layer, second tunneling oxide layer, N-polysilicon layer and first tunneling oxide layer on the second surface are removed by RCA cleaning. Finally, a 6nm aluminum oxide passivation layer is deposited on the second surface of the silicon wafer by ALD, a 75nm SiNx first anti-reflection film layer is deposited by PE, and a 90nm SiNx second anti-reflection layer is deposited on the back by PE. Finally, metal electrodes are formed on the surfaces of both sides of the battery structure formed by the above steps by screen printing using a 16-sub-gate pattern structure, a sintering furnace and a Leco laser.
[0131] Use a battery efficiency tester to test the electrical performance of photovoltaic cells.
[0132] Example 4
[0133] The difference from Example 3 is that in step 102: the first tunneling oxide layer and the second tunneling oxide layer are both prepared by thermal oxidation; wherein the gas flow rate of the first tunneling oxide layer is 30000sccm, the temperature is 580°C, the pressure is 600mtorr, and the process time is 2min; the gas flow rate of the first tunneling oxide layer is 30000sccm, the temperature is 580°C, the pressure is 600mtorr, and the process time is 1min.
[0134] Example 5
[0135] The difference from Example 3 is that in step 102: the first tunnel oxide layer is prepared by thermal oxidation; wherein the gas flow rate is 30000 sccm, the temperature is 580° C., the pressure is 600 mtorr, and the process time is 2 min.
[0136] Example 6
[0137] The difference from Example 3 is that in step 102, a second amorphous silicon layer is finally deposited, the temperature is maintained at 580°C, and then SiH4 is introduced at a flow rate of 1300sccm, a pressure of 180mtorr, and a process time of 30min.
[0138] Comparative Example 4
[0139] Step 101: Select an N-type single crystal silicon wafer, the resistivity of the silicon wafer is 0.5-2Ω·cm, the size of the silicon wafer is 182×182mm, the thickness is 130μm, and the surface of the silicon wafer is subjected to alkali texturing treatment;
[0140] Step 102: depositing a tunneling oxide layer and an amorphous silicon layer in sequence on the surface of the silicon wafer;
[0141] First, the tunnel oxide layer was deposited by thermal oxidation with a gas flow rate of 40,000 sccm, a temperature of 580°C, a pressure of 600 mtorr, and a process time of 5 min.
[0142] Then the temperature was raised to 610°C to deposit an amorphous silicon layer, with a SiH4 flow rate of 1600 sccm, a temperature of 610°C, a pressure of 180 mtorr, and a process time of 40 min.
[0143] Step 103: performing high temperature diffusion to form a passivation layer;
[0144] Among them, the amorphous silicon layer is subjected to boron diffusion and annealing by high-temperature thermal diffusion, and boron trichloride is selected as the doping source. The doping source flow rate of the source step is 160sccm, the pressure is 120bar, the temperature is 800-850℃, and the time is 300 seconds. The pressure of the annealing step is 300bar, the temperature is 940℃, and the process time is 1200 seconds.
[0145] The final passivation layer is composed of a tunneling oxide layer and a P-type doped polysilicon layer. The thicknesses of the tunneling oxide layer and the P-type doped polysilicon layer are 1.5 nm and 160 nm respectively. The doping concentration of the P-type doped polysilicon layer is 4.45×10 19 / cm3.
[0146] Subsequently, the PSG layer, the P+ polysilicon layer and the tunnel oxide layer on the second surface are removed by RCA cleaning, and finally a 6nm aluminum oxide passivation layer 3 is deposited on the second surface of the silicon wafer 1 by ALD, a 75nm SiNx first anti-reflection film layer is deposited by PE, and a 90nm SiNx second anti-reflection layer is deposited on the first surface by PE; finally, metal electrodes are formed on the surfaces of both sides of the battery structure formed by the above steps by screen printing using a 16-sub-gate pattern structure, a sintering furnace and a Leco laser.
[0147] Table 2 below shows the test data of Examples 3-6 and Comparative Example 4, where Eta is the battery efficiency, Voc is the open circuit voltage, Isc is the current density, FF is the fill factor, Rs is the series resistance, Rsh is the parallel resistance, and Irev2 is the leakage current. As can be seen from the table, (1) Compared with Comparative Example 4, the efficiency Eta of Example 3 is significantly increased, its Uoc, Isc and FF are all increased, and Irev2 is also reduced. (2) Compared with Example 3 and Comparative Example 4, Example 4 uses thermal oxidation to prepare the passivation layer, and Example 5 uses the first tunneling oxide layer thermal oxidation and the second tunneling oxide layer thermal oxidation to prepare the passivation layer. Although its efficiency is slightly higher than that of Comparative Example 4, its electrical performance data is still somewhat different from that of Example 3. (3) Compared with Example 3. Example 6 uses the same temperature to prepare the first amorphous silicon layer and the second amorphous silicon layer. Since the low-temperature deposited polycrystalline silicon layer has a poor effect on blocking the internal expansion of the doped elements in the tunneling oxide layer during subsequent diffusion, it affects the passivation effect of the tunneling oxide layer. Therefore, its electrical performance data is also somewhat different from that of Example 3.
[0148] Table 2 Test data of Examples 3-6 and Comparative Example 4
[0149]
[0150] Although the present application is described herein in conjunction with various embodiments, in the process of implementing the claimed application, those skilled in the art may understand and implement other changes to the disclosed embodiments by viewing the drawings, the disclosure, and the appended claims. In the claims, the word "comprising" does not exclude other components or steps, and "one" or "an" does not exclude multiple situations. A single processor or other unit may implement several functions listed in a claim. Certain measures are recorded in different dependent claims, but this does not mean that these measures cannot be combined to produce good results.
[0151] Although the present application has been described in conjunction with specific features and embodiments thereof, it is obvious that various modifications and combinations may be made thereto without departing from the spirit and scope of the present application. Accordingly, this specification and the drawings are merely exemplary illustrations of the present application as defined by the appended claims, and are deemed to have covered any and all modifications, variations, combinations or equivalents within the scope of the present application. Obviously, those skilled in the art may make various modifications and variations to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application fall within the scope of the claims of the present application and their equivalents, the present application is also intended to include these modifications and variations.
Claims
1. A method for preparing a photovoltaic cell, characterized in that: The following steps are involved: Step 101: Select a silicon wafer and perform a texturing process on the silicon wafer; the silicon wafer is an N-type single crystal silicon wafer; Step 102: depositing a first tunneling oxide layer, a first amorphous silicon layer, a second tunneling oxide layer, and a second amorphous silicon layer in sequence on the surface of the silicon wafer; wherein: Depositing the first tunnel oxide layer and the second tunnel oxide layer by LPCVD; Depositing the first amorphous silicon layer and the second amorphous silicon layer by LPCVD; The first tunneling oxide layer is deposited by first thermal oxidation and then water oxygen; wherein the flow rate of oxygen carried in the thermal oxidation process is 10000sccm to 50000sccm; the flow rate of oxygen carried in the water oxygen process is 100sccm to 1000sccm; the time of thermal oxygen deposition is 1min to 30min; the time of water oxygen deposition is 1min to 10min; the deposition temperature of thermal oxygen is 500 to 700°C; the deposition temperature of water oxygen is 500 to 600°C; The deposition temperature of the first amorphous silicon layer is 500-600° C.; the gas flow rate of the first amorphous silicon layer is 1000 sccm-2000 sccm; the deposition time of the first amorphous silicon layer is 1 min-15 min; The second tunneling oxide layer is prepared by a water-oxygen method; the oxygen flow rate carried by the water-oxygen is 100-1000 sccm, and the nitrogen flow rate is 1000-5000 sccm; the deposition temperature is 500-600° C., and the water-oxygen deposition time is 1 min-10 min; The deposition temperature of the first amorphous silicon layer is lower than the deposition temperature of the second amorphous silicon layer, the gas flow rate when depositing the first amorphous silicon layer is greater than the gas flow rate when depositing the second amorphous silicon layer; the deposition time of the first amorphous silicon layer is less than the deposition time of the second amorphous silicon layer; the deposition temperature of the second amorphous silicon layer is 500-700° C.; the gas flow rate when depositing the second amorphous silicon layer is 1000 sccm-2000 sccm; the deposition time of the second amorphous silicon layer is 10 min-30 min; Step 103: Perform high temperature diffusion to form a passivation layer. The formed passivation layer includes the first tunneling oxide layer, the first doped polysilicon layer, the second tunneling oxide layer and the second doped polysilicon layer in sequence on the first surface of the silicon wafer; The first doped polysilicon layer and the second doped polysilicon layer have the same doping type, the doping concentration of the first doped polysilicon layer is less than the doping concentration of the second doped polysilicon layer, and when the doping type is N-type, the doping concentration of the first doped polysilicon layer is 1-2.5×10 20 / cm 3 The doping concentration of the second doped polysilicon layer is 3-5×10 20 / cm 3 When the doping type is P type, the doping concentration of the first doped polysilicon layer is 2-4×10 19 / cm 3 The doping concentration of the second doped polysilicon layer is 4-5×10 19 / cm 3 ; The thickness of the first doped polysilicon layer is less than the thickness of the second doped polysilicon layer; the thickness of the first doped polysilicon layer is 10-80 nm; the thickness of the second doped polysilicon layer is 50-150 nm; The thickness of the first tunneling oxide layer is greater than the thickness of the second tunneling oxide layer; the thickness of the first tunneling oxide layer is 1.5-2 nm, and the thickness of the second tunneling oxide layer is 1-1.5 nm.
2. The method for preparing a photovoltaic cell according to claim 1, characterized in that: The resistivity of the silicon wafer is 0.5-2Ω·cm.
3. A photovoltaic cell, characterized in that: A photovoltaic cell prepared by the preparation method according to any one of claims 1-2.
4. A photovoltaic module, characterized in that: A photovoltaic cell comprising the photovoltaic cell of claim 3.