Environmentally friendly self-cleaning building material and preparation method thereof

By introducing superhydrophobic polyvinylidene fluoride membranes and modified fluorocarbon resins into environmentally friendly building materials, the problem of these materials being easily contaminated has been solved, and their self-cleaning properties and mechanical properties have been improved.

CN118515453BActive Publication Date: 2024-11-05NANTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410977668.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-05
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Existing environmentally friendly building materials are easily contaminated when exposed to the external environment, affecting their lifespan and aesthetics, and lack self-cleaning properties.

Method used

The method employs a combination of materials such as superhydrophobic polyvinylidene fluoride membrane, modified fluorocarbon resin, polycarbonate, cement, cellulose sulfonate water-reducing agent, and epoxy nano silica. By mixing and casting, the method utilizes the hydrophobic and self-cleaning properties of the materials to achieve anti-fouling and self-cleaning effects.

Benefits of technology

It improves the stain resistance and self-cleaning properties of environmentally friendly building materials, enhances their mechanical properties, extends their service life, and maintains their aesthetic appeal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of environmentally friendly self-cleaning building materials, and discloses an environmentally friendly self-cleaning building material and a preparation method thereof. Raw materials are stirred and mixed according to a proportion, then poured into a mold, cured, and demolded to obtain the environmentally friendly self-cleaning building material. The fluorocarbon acrylic resin in the modified fluorocarbon resin has extremely low surface energy and super strong hydrophobicity and oleophobicity, thereby achieving a self-cleaning effect. Graphene, silicone rubber, and polycarbonate themselves have a self-cleaning effect, and together play an anti-fouling effect on the environmentally friendly building material. During the pouring process, the epoxy group of epoxy nano-silica will undergo a ring-opening reaction with the carboxyl group of the modified fluorocarbon resin to obtain an organic silicone resin, which has a lower surface free energy and better hydrophobicity and oleophobicity, and has a better anti-fouling effect on the environmentally friendly building material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmentally friendly self-cleaning building materials, in particular to an environmentally friendly self-cleaning building material and a preparation method thereof. Background Art

[0002] Environmentally friendly building materials pay more attention to environmental protection during the design and production process. Environmentally friendly building materials include brick materials, concrete materials, wood, soil building materials, etc. The use of environmentally friendly building materials can reduce the use of natural materials and reduce the pollution of construction to the environment. However, building materials are exposed to the air all year round and are always subject to various external pollution, which affects their lifespan and appearance. How to apply anti-fouling and self-cleaning technology to environmentally friendly building materials is the key to solving the problem.

[0003] Silicone rubber has excellent softness and can be bent up to tens of thousands of times. Silicone rubber also has hydrophobic properties. Water will spontaneously form water droplets on the hydrophobic surface. When the water droplets roll on the inclined surface, they will spontaneously carry away some particles attached to the surface, achieving self-cleaning. The graphene surface can automatically remove dirt and bacteria and can remain clean even without detergent. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the deficiencies in the prior art, the present invention provides an environmentally friendly self-cleaning building material and a preparation method thereof, which has good environmental protection and self-cleaning properties.

[0006] (II) Technical solution

[0007] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: an environmentally friendly self-cleaning building material, which comprises the following components by weight: 5-8 parts by weight of super-hydrophobic polyvinylidene fluoride film, 3-15 parts by weight of modified fluorocarbon resin, 12-20 parts by weight of polycarbonate, 40-60 parts by weight of cement, 0.2-0.5 parts by weight of cellulose sulfonate water reducer, 10-30 parts by weight of water, and 0.5-1 parts by weight of epoxy nano-silica.

[0008] Preferably, the preparation method of the polyvinylidene fluoride is:

[0009] (1) Add 8-15 parts by weight of polyvinylidene fluoride to N,N-dimethylformamide solvent, stir at 60-80°C for 1-2h, degas for 20-40min, dry at 120-140°C, bake for 3-5min, and then treat with oxygen plasma at a vacuum degree of 8-10Pa for 5-15min at a treatment power of 180-200W to obtain intermediate product A;

[0010] (2) 10-14 parts by weight of methyltrichlorosilane is dissolved in toluene solvent, and then placed in a container with a relative humidity of 30-70%, and 10-13 parts by weight of intermediate product A is added to the container for immersion for 10-20 minutes to obtain a superhydrophobic polyvinylidene fluoride film.

[0011] Preferably, the preparation method of the modified fluorocarbon resin is:

[0012] S1. Add dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent into a reactor, stir for 1-2 hours, introduce argon for 0.5-0.6 hours, react at 30-40° C. for 3-6 hours, remove the solvent by distillation under reduced pressure, filter and dry to obtain a modified acrylic resin;

[0013] S2. Add graphene oxide to N,N-dimethylformamide solvent, stir evenly, then add hexamethylene diisocyanate and dibutyltin disilicate catalyst, introduce nitrogen protection, react at 70-90° C. for 4-8 hours, then continue to add 4-fluoroisoglutamide, react at 60-100° C. for 10-15 hours, distill under reduced pressure after the reaction, filter and wash to obtain modified graphene;

[0014] S3. Add modified acrylic resin and modified graphene into the reactor, stir evenly, slowly drop dibutyltin dilaurate catalyst, wash with acetone, precipitate for 2-4 hours, filter, and obtain modified fluorocarbon resin.

[0015] Preferably, the mass ratio of dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber and TPO photoinitiator in S1 is 1.2-1.6:1:0.8-1.5:1:0.1-0.3.

[0016] Preferably, the preparation method of the olefinic silicone rubber in S1 is:

[0017] S4. Add methanol solvent, polymerization inhibitor butylated hydroxytoluene, catalyst chloroplatinic acid tetrahydrofuran solution, and dipropylene glycol diacrylate into the reactor, ultrasonically disperse for 20-30 minutes, then add silicone rubber, react at 40-70°C for 3-6 hours, cool, centrifuge, and wash to obtain olefinic silicone rubber.

[0018] Preferably, the mass ratio of the polymerization inhibitor butylated hydroxytoluene, the catalyst chloroplatinic acid, the dipropylene glycol diacrylate, and the silicone rubber in S4 is 0.01-0.03:0.02-0.04:1.2-1.5:1.3-1.6.

[0019] Preferably, the mass ratio of graphene oxide, hexamethylene diisocyanate, dibutyltin diisocyanate catalyst and 4-fluoroisoglutamide in S2 is 2.1-2.6:1.8-2.4:0.1-0.3:1.1-1.3.

[0020] Preferably, the mass ratio of the modified acrylic resin, the modified graphene, and the dibutyltin dilaurate catalyst in S3 is 1:1.2-1.4:0.01-0.03.

[0021] Preferably, the preparation method of the environmentally friendly self-cleaning building material comprises the following steps: mixing super-hydrophobic polyvinylidene fluoride film, modified fluorocarbon resin, polycarbonate, cement, cellulose sulfonate water reducer, water, and epoxy nano-silica according to a ratio, then pouring them into a mold, curing for 6-10 days, and demolding to obtain the environmentally friendly self-cleaning building material.

[0022] 3. Beneficial technical effects

[0023] The invention prepares an environmentally friendly self-cleaning building material by stirring and mixing a super-hydrophobic polyvinylidene fluoride film, a modified fluorocarbon resin, polycarbonate, cement, a cellulose sulfonate water reducing agent, water and epoxy nano-silica, then pouring the mixture into a mold, performing curing and demoulding.

[0024] After the polyvinylidene fluoride is treated with oxygen plasma, methyltrichlorosilane is introduced for surface deposition treatment to obtain a super-hydrophobic polyvinylidene fluoride film, which has a low surface energy and good hydrophobicity. It can be used in environmentally friendly building materials to achieve anti-fouling and self-cleaning effects; the fluorocarbon acrylic resin in the modified fluorocarbon resin has extremely low surface energy and super strong hydrophobicity and oleophobicity, thereby achieving a self-cleaning effect. Graphene, silicone rubber and polycarbonate themselves have self-cleaning effects, and together they have an anti-fouling effect on environmentally friendly building materials. Graphene can also increase the toughness and tensile strength of polycarbonate, thereby enhancing the mechanical properties of environmentally friendly self-cleaning building materials; during the casting process, the epoxy group of epoxy nano-silica will undergo a ring-opening reaction with the carboxyl group of the modified fluorocarbon resin to obtain an organic silicone resin with a low surface free energy and good hydrophobicity and oleophobicity, which has a good anti-fouling effect on environmentally friendly building materials. DETAILED DESCRIPTION

[0025] Epoxy Nano-Silica (Existing Technology) Example 1

[0026] (1) Add 8 parts by weight of polyvinylidene fluoride to N,N-dimethylformamide solvent, stir at 60°C for 1 hour, degas for 20 minutes, dry at 120°C, bake for 3 minutes, and then treat with oxygen plasma at a vacuum degree of 8 Pa for 5 minutes at a treatment power of 180 W to obtain intermediate product A;

[0027] (2) dissolving 10 parts by weight of methyltrichlorosilane in a toluene solvent, placing the solvent in a container at a relative humidity of 30%, adding 10 parts by weight of the intermediate product A into the container for immersion for 10 minutes, and obtaining a super-hydrophobic polyvinylidene fluoride film;

[0028] (3) Adding methanol solvent, polymerization inhibitor butylated hydroxytoluene, tetrahydrofuran solution of chloroplatinic acid catalyst, and dipropylene glycol diacrylate into the reactor, wherein the mass ratio of polymerization inhibitor butylated hydroxytoluene, catalyst chloroplatinic acid, dipropylene glycol diacrylate, and silicone rubber is 0.01:0.02:1.2:1.3, ultrasonically dispersing for 20 minutes, then adding silicone rubber, reacting at 40°C for 3 hours, cooling, centrifuging, and washing to obtain olefinic silicone rubber;

[0029] (4) Add dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent into a reactor, wherein the mass ratio of dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent is 1.2:1:0.8:1:0.1, stir for 1 hour, introduce argon for 0.5 hour, react at 30° C. for 3 hours, remove the solvent by distillation under reduced pressure, filter and dry to obtain a modified acrylic resin;

[0030] (5) Adding graphene oxide to N,N-dimethylformamide solvent, stirring evenly, then adding hexamethylene diisocyanate and dibutyltin diisocyanate catalyst, introducing nitrogen protection, reacting at 70°C for 4 hours, and then continuing to add 4-fluoroisoglutamide, wherein the mass ratio of graphene oxide, hexamethylene diisocyanate, dibutyltin diisocyanate catalyst, and 4-fluoroisoglutamide is 2.1:1.8:0.1:1.1, reacting at 60°C for 10 hours, and after the reaction, distilling under reduced pressure, filtering, and washing to obtain modified graphene;

[0031] (6) Adding modified acrylic resin and modified graphene into a reactor, stirring evenly, slowly adding dibutyltin dilaurate catalyst dropwise, wherein the mass ratio of modified acrylic resin, modified graphene and dibutyltin dilaurate catalyst is 1:1.2:0.01, washing with acetone, precipitating for 2 hours, filtering, and obtaining modified fluorocarbon resin;

[0032] (7) 5 parts by weight of super-hydrophobic polyvinylidene fluoride film, 3 parts by weight of modified fluorocarbon resin, 12 parts by weight of polycarbonate, 40 parts by weight of cement, 0.2 parts by weight of cellulose sulfonate water reducer, 10 parts by weight of water, and 0.5 parts by weight of epoxy nano-silica were stirred and mixed, then poured into a mold, cured for 6 days, and demolded to obtain an environmentally friendly self-cleaning building material. Example 2

[0033] (1) Add 15 parts by weight of polyvinylidene fluoride to N,N-dimethylformamide solvent, stir at 80°C for 2 hours, degas for 40 minutes, dry at 140°C, bake for 5 minutes, and then treat with oxygen plasma at a vacuum degree of 10 Pa for 15 minutes at a processing power of 200 W to obtain intermediate product A;

[0034] (2) dissolving 10 parts by weight of methyltrichlorosilane in a toluene solvent, placing the solvent in a container at a relative humidity of 30%, adding 10 parts by weight of the intermediate product A into the container for immersion for 10 minutes, and obtaining a super-hydrophobic polyvinylidene fluoride film;

[0035] (3) Adding methanol solvent, polymerization inhibitor butylated hydroxytoluene, tetrahydrofuran solution of chloroplatinic acid catalyst, and dipropylene glycol diacrylate into the reactor, wherein the mass ratio of polymerization inhibitor butylated hydroxytoluene, catalyst chloroplatinic acid, dipropylene glycol diacrylate, and silicone rubber is 0.01:0.02:1.2:1.3, ultrasonically dispersing for 20 minutes, then adding silicone rubber, reacting at 40°C for 3 hours, cooling, centrifuging, and washing to obtain olefinic silicone rubber;

[0036] (4) Add dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent into a reactor, wherein the mass ratio of dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent is 1.2:1:0.8:1:0.1, stir for 1 hour, introduce argon for 0.5 hour, react at 30° C. for 3 hours, remove the solvent by distillation under reduced pressure, filter and dry to obtain a modified acrylic resin;

[0037] (5) Adding graphene oxide to N,N-dimethylformamide solvent, stirring evenly, then adding hexamethylene diisocyanate and dibutyltin diisocyanate catalyst, introducing nitrogen protection, reacting at 70°C for 4 hours, and then continuing to add 4-fluoroisoglutamide, wherein the mass ratio of graphene oxide, hexamethylene diisocyanate, dibutyltin diisocyanate catalyst, and 4-fluoroisoglutamide is 2.1:1.8:0.1:1.1, reacting at 60°C for 10 hours, and after the reaction, distilling under reduced pressure, filtering, and washing to obtain modified graphene;

[0038] (6) Adding modified acrylic resin and modified graphene into a reactor, stirring evenly, slowly adding dibutyltin dilaurate catalyst dropwise, wherein the mass ratio of modified acrylic resin, modified graphene and dibutyltin dilaurate catalyst is 1:1.2:0.01, washing with acetone, precipitating for 2 hours, filtering, and obtaining modified fluorocarbon resin;

[0039] (7) 5 parts by weight of super-hydrophobic polyvinylidene fluoride film, 3 parts by weight of modified fluorocarbon resin, 12 parts by weight of polycarbonate, 40 parts by weight of cement, 0.2 parts by weight of cellulose sulfonate water reducer, 10 parts by weight of water, and 0.5 parts by weight of epoxy nano-silica were stirred and mixed, then poured into a mold, cured for 6 days, and demolded to obtain an environmentally friendly self-cleaning building material. Example 3

[0040] (1) Add 11.5 parts by weight of polyvinylidene fluoride to N,N-dimethylformamide solvent, stir at 70°C for 1.5 hours, degas for 30 minutes, dry at 130°C, bake for 4 minutes, and then treat with oxygen plasma at a vacuum degree of 9 Pa for 10 minutes at a treatment power of 190 W to obtain intermediate product A;

[0041] (2) dissolving 12 parts by weight of methyltrichlorosilane in a toluene solvent, placing the solvent in a container at a relative humidity of 50%, adding 11.5 parts by weight of the intermediate product A into the container for immersion for 15 minutes, and obtaining a super-hydrophobic polyvinylidene fluoride film;

[0042] (3) Adding methanol solvent, polymerization inhibitor butylated hydroxytoluene, tetrahydrofuran solution of chloroplatinic acid catalyst, and dipropylene glycol diacrylate into the reactor, wherein the mass ratio of polymerization inhibitor butylated hydroxytoluene, catalyst chloroplatinic acid, dipropylene glycol diacrylate, and silicone rubber is 0.02:0.03:1.35:1.45, ultrasonically dispersing for 25 minutes, then adding silicone rubber, reacting at 55°C for 4.5 hours, cooling, centrifuging, and washing to obtain olefinic silicone rubber;

[0043] (4) Add dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent into a reactor, wherein the mass ratio of dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent is 1.4:1:1.15:1:0.2, stir for 1.5 hours, introduce argon for 0.55 hours, react at 35°C for 4.5 hours, remove the solvent by distillation under reduced pressure, filter and dry to obtain a modified acrylic resin;

[0044] (5) Adding graphene oxide to N,N-dimethylformamide solvent, stirring evenly, then adding hexamethylene diisocyanate and dibutyltin diisocyanate catalyst, passing nitrogen protection, reacting at 80°C for 6 hours, and then continuing to add 4-fluoroisoglutamide, wherein the mass ratio of graphene oxide, hexamethylene diisocyanate, dibutyltin diisocyanate catalyst, and 4-fluoroisoglutamide is 2.35:2.1:0.2:1.2, reacting at 80°C for 12.5 hours, and after the reaction, distilling under reduced pressure, filtering, and washing to obtain modified graphene;

[0045] (6) Add the modified acrylic resin and modified graphene into the reactor, stir evenly, and slowly drop the dibutyl tin dilaurate catalyst, wherein the mass ratio of the modified acrylic resin, modified graphene, and dibutyl tin dilaurate catalyst is 1:1.3:0.02. After completion, wash with acetone, precipitate for 3 hours, and filter to obtain the modified fluorocarbon resin.

[0046] (7) 6.5 parts by weight of super-hydrophobic polyvinylidene fluoride film, 9 parts by weight of modified fluorocarbon resin, 16 parts by weight of polycarbonate, 50 parts by weight of cement, 0.35 parts by weight of cellulose sulfonate water reducer, 20 parts by weight of water, and 0.8 parts by weight of epoxy nano-silica were stirred and mixed, then poured into a mold, cured for 8 days, and demolded to obtain an environmentally friendly self-cleaning building material. Example 4

[0047] (1) Add 8 parts by weight of polyvinylidene fluoride to N,N-dimethylformamide solvent, stir at 60°C for 1 hour, degas for 20 minutes, dry at 120°C, bake for 3 minutes, and then treat with oxygen plasma at a vacuum degree of 8 Pa for 5 minutes at a treatment power of 180 W to obtain intermediate product A;

[0048] (2) dissolving 10 parts by weight of methyltrichlorosilane in a toluene solvent, placing the solvent in a container at a relative humidity of 30%, adding 10 parts by weight of the intermediate product A into the container for immersion for 10 minutes, and obtaining a super-hydrophobic polyvinylidene fluoride film;

[0049] (3) Adding methanol solvent, polymerization inhibitor butylated hydroxytoluene, tetrahydrofuran solution of chloroplatinic acid catalyst, and dipropylene glycol diacrylate into the reactor, wherein the mass ratio of polymerization inhibitor butylated hydroxytoluene, catalyst chloroplatinic acid, dipropylene glycol diacrylate, and silicone rubber is 0.01:0.02:1.2:1.3, ultrasonically dispersing for 20 minutes, then adding silicone rubber, reacting at 40°C for 3 hours, cooling, centrifuging, and washing to obtain olefinic silicone rubber;

[0050] (4) Add dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent into a reactor, wherein the mass ratio of dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent is 1.2:1:0.8:1:0.1, stir for 1 hour, introduce argon for 0.5 hour, react at 30° C. for 3 hours, remove the solvent by distillation under reduced pressure, filter and dry to obtain a modified acrylic resin;

[0051] (5) Adding graphene oxide to N,N-dimethylformamide solvent, stirring evenly, then adding hexamethylene diisocyanate and dibutyltin diisocyanate catalyst, passing nitrogen protection, reacting at 80°C for 6 hours, and then continuing to add 4-fluoroisoglutamide, wherein the mass ratio of graphene oxide, hexamethylene diisocyanate, dibutyltin diisocyanate catalyst, and 4-fluoroisoglutamide is 2.35:2.1:0.2:1.2, reacting at 80°C for 12.5 hours, and after the reaction, distilling under reduced pressure, filtering, and washing to obtain modified graphene;

[0052] (6) Add the modified acrylic resin and modified graphene into the reactor, stir evenly, and slowly drop the dibutyl tin dilaurate catalyst, wherein the mass ratio of the modified acrylic resin, modified graphene, and dibutyl tin dilaurate catalyst is 1:1.3:0.02. After completion, wash with acetone, precipitate for 3 hours, and filter to obtain the modified fluorocarbon resin.

[0053] (7) 6.5 parts by weight of super-hydrophobic polyvinylidene fluoride film, 9 parts by weight of modified fluorocarbon resin, 16 parts by weight of polycarbonate, 50 parts by weight of cement, 0.35 parts by weight of cellulose sulfonate water reducer, 20 parts by weight of water, and 0.8 parts by weight of epoxy nano-silica were stirred and mixed, then poured into a mold, cured for 8 days, and demolded to obtain an environmentally friendly self-cleaning building material. Example 5

[0054] (1) Add 15 parts by weight of polyvinylidene fluoride to N,N-dimethylformamide solvent, stir at 80°C for 2 hours, degas for 40 minutes, dry at 140°C, bake for 5 minutes, and then treat with oxygen plasma at a vacuum degree of 10 Pa for 15 minutes at a processing power of 200 W to obtain intermediate product A;

[0055] (2) dissolving 10 parts by weight of methyltrichlorosilane in a toluene solvent, placing the solvent in a container at a relative humidity of 30%, adding 10 parts by weight of the intermediate product A into the container for immersion for 10 minutes, and obtaining a super-hydrophobic polyvinylidene fluoride film;

[0056] (3) Adding methanol solvent, polymerization inhibitor butylated hydroxytoluene, tetrahydrofuran solution of chloroplatinic acid catalyst, and dipropylene glycol diacrylate into the reactor, wherein the mass ratio of polymerization inhibitor butylated hydroxytoluene, catalyst chloroplatinic acid, dipropylene glycol diacrylate, and silicone rubber is 0.02:0.03:1.35:1.45, ultrasonically dispersing for 25 minutes, then adding silicone rubber, reacting at 55°C for 4.5 hours, cooling, centrifuging, and washing to obtain olefinic silicone rubber;

[0057] (4) Add dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent into a reactor, wherein the mass ratio of dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent is 1.4:1:1.15:1:0.2, stir for 1.5 hours, introduce argon for 0.55 hours, react at 35°C for 4.5 hours, remove the solvent by distillation under reduced pressure, filter and dry to obtain a modified acrylic resin;

[0058] (5) Adding graphene oxide to N,N-dimethylformamide solvent, stirring evenly, then adding hexamethylene diisocyanate and dibutyltin diisocyanate catalyst, introducing nitrogen protection, reacting at 70°C for 4 hours, and then continuing to add 4-fluoroisoglutamide, wherein the mass ratio of graphene oxide, hexamethylene diisocyanate, dibutyltin diisocyanate catalyst, and 4-fluoroisoglutamide is 2.1:1.8:0.1:1.1, reacting at 60°C for 10 hours, and after the reaction, distilling under reduced pressure, filtering, and washing to obtain modified graphene;

[0059] (6) Adding modified acrylic resin and modified graphene into a reactor, stirring evenly, slowly adding dibutyltin dilaurate catalyst dropwise, wherein the mass ratio of modified acrylic resin, modified graphene and dibutyltin dilaurate catalyst is 1:1.2:0.01, washing with acetone, precipitating for 2 hours, filtering, and obtaining modified fluorocarbon resin;

[0060] (7) 5 parts by weight of super-hydrophobic polyvinylidene fluoride film, 3 parts by weight of modified fluorocarbon resin, 12 parts by weight of polycarbonate, 40 parts by weight of cement, 0.2 parts by weight of cellulose sulfonate water reducer, 10 parts by weight of water, and 0.5 parts by weight of epoxy nano-silica were stirred and mixed, then poured into a mold, cured for 6 days, and demolded to obtain an environmentally friendly self-cleaning building material.

[0061] Comparative Example 1

[0062] 12 parts by weight of polycarbonate, 40 parts by weight of cement, 0.2 parts by weight of cellulose sulfonate water reducer, 10 parts by weight of water, and 0.5 parts by weight of epoxy nano-silica were stirred and mixed, then poured into a mold, cured for 6 days, and demolded to obtain an environmentally friendly self-cleaning building material.

[0063] According to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the compressive strength test of the environmentally friendly self-cleaning building materials of Examples 1-5 and Comparative Example 1 was carried out; the environmentally friendly self-cleaning building materials of Examples 1-5 and Comparative Example 1 were naturally placed for 20 days, and the self-cleaning degree was observed; the size of the environmentally friendly self-cleaning building materials for the compressive strength test and the self-cleaning degree test was 100mm×100mm×100mm.

[0064] Table 1: Compressive strength test and self-cleaning test.

[0065]

[0066] It can be seen from Table 1 that the environmentally friendly self-cleaning building material of the present invention has good compression resistance and self-cleaning performance.

[0067] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. An environmentally friendly self-cleaning building material, It is characterized in that The environmentally friendly self-cleaning building material comprises the following components by weight: 5-8 parts by weight of super-hydrophobic polyvinylidene fluoride film, 3-15 parts by weight of modified fluorocarbon resin, 12-20 parts by weight of polycarbonate, 40-60 parts by weight of cement, 0.2-0.5 parts by weight of cellulose sulfonate water reducer, 10-30 parts by weight of water, and 0.5-1 parts by weight of epoxy nano-silica; The preparation method of the modified fluorocarbon resin is: S1. Add dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator, and ethyl acetate solvent into a reactor, stir for 1-2 hours, introduce argon for 0.5-0.6 hours, react at 30-40° C. for 3-6 hours, remove the solvent by distillation under reduced pressure, filter and dry to obtain a modified acrylic resin; S2. Add graphene oxide to N,N-dimethylformamide solvent, stir evenly, then add hexamethylene diisocyanate and dibutyltin disilicate catalyst, introduce nitrogen protection, react at 70-90° C. for 4-8 hours, then continue to add 4-fluoroisoglutamide, react at 60-100° C. for 10-15 hours, distill under reduced pressure after the reaction, filter and wash to obtain modified graphene; S3. Add modified acrylic resin and modified graphene into the reactor, stir evenly, slowly drop dibutyltin dilaurate catalyst, wash with acetone, precipitate for 2-4 hours, filter, and obtain modified fluorocarbon resin.

2. The environmentally friendly self-cleaning building material according to claim 1, It is characterized in that The preparation method of the super hydrophobic polyvinylidene fluoride film is: (1) Add 8-15 parts by weight of polyvinylidene fluoride to N,N-dimethylformamide solvent, stir at 60-80°C for 1-2h, degas for 20-40min, dry at 120-140°C, bake for 3-5min, and then treat with oxygen plasma at a vacuum degree of 8-10Pa for 5-15min at a treatment power of 180-200W to obtain intermediate product A; (2) 10-14 parts by weight of methyltrichlorosilane is dissolved in toluene solvent, and then placed in a container with a relative humidity of 30-70%, and 10-13 parts by weight of intermediate product A is added to the container for immersion for 10-20 minutes to obtain a superhydrophobic polyvinylidene fluoride film.

3. The environmentally friendly self-cleaning building material according to claim 1, It is characterized in that The mass ratio of dipropylene glycol diacrylate, methyl methacrylate, olefinic silicone rubber, TPO photoinitiator and ethyl acetate solvent in S1 is 1.2-1.6:1:0.8-1.5:1:0.1-0.

3.

4. The environmentally friendly self-cleaning building material according to claim 1, It is characterized in that The preparation method of the olefinic silicone rubber in S1 is: S4. Add methanol solvent, polymerization inhibitor butylated hydroxytoluene, catalyst chloroplatinic acid tetrahydrofuran solution, and dipropylene glycol diacrylate into the reactor, ultrasonically disperse for 20-30 minutes, then add silicone rubber, react at 40-70°C for 3-6 hours, cool, centrifuge, and wash to obtain olefinic silicone rubber.

5. The environmentally friendly self-cleaning building material according to claim 4, It is characterized in that The mass ratio of the polymerization inhibitor dibutyl hydroxytoluene, the catalyst chloroplatinic acid, the dipropylene glycol diacrylate, and the silicone rubber in the S4 is 0.01-0.03:0.02-0.04:1.2-1.5:1.3-1.

6.

6. The environmentally friendly self-cleaning building material according to claim 1, It is characterized in that The mass ratio of graphene oxide, hexamethylene diisocyanate, dibutyltin diisocyanate catalyst and 4-fluoroisoglutamide in S2 is 2.1-2.6:1.8-2.4:0.1-0.3:1.1-1.

3.

7. The environmentally friendly self-cleaning building material according to claim 1, It is characterized in that The mass ratio of the modified acrylic resin, the modified graphene and the dibutyltin dilaurate catalyst in S3 is 1:1.2-1.4:0.01-0.

03.

8. A method for preparing the environmentally friendly self-cleaning building material according to any one of claims 1 to 7, It is characterized in that The preparation method of the environmentally friendly self-cleaning building material comprises the following steps: mixing super-hydrophobic polyvinylidene fluoride film, modified fluorocarbon resin, polycarbonate, cement, cellulose sulfonate water reducer, water and epoxy nano-silica according to a proportion, then pouring them into a mold, curing for 6-10 days, and demolding to obtain the environmentally friendly self-cleaning building material.