A method for smelting and separating high-lead molybdenum concentrate
Through the combination of high-temperature smelting and alkali leaching steps of molybdenum iron concentrate, the problem of difficult control of lead content in molybdenum concentrate is solved, the effective reduction of molybdenum lead separation and the guarantee of quality of molybdenum iron product is achieved, and the operation is simplified and production is improved. Practicality.
Patent Information
- Application Number
- CN202410568213.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-05-08
AI Technical Summary
The lead content in existing molybdenum concentrates is difficult to effectively control, especially in small mines and ore dressing processes. Traditional methods have problems with the risk of toxic substance use and high cost.
The volatile characteristics of lead are separated by high-temperature smelting of molybdenum iron, combined with oxidation and roasting and alkali leaching steps, the separation of molybdenum lead is achieved, and the low-molybdenum high-lead dust collection powder is used for deep processing, and the weak alkaline macroporous ion exchange resin is used for molybdenum enrichment. and impurities removal.
It realizes effective control of molybdenum-lead separation, ensures the quality of molybdenum-ferrous molybdenum product, reduces the lead content, simplifies the operation process, and improves the practicality and safety of production.
Smart Images

Figure CN118516570B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of molybdenum smelting, and specifically discloses a method for smelting and separating high-lead molybdenum concentrate. Background Art
[0002] Lead and iron are difficult to form solid solutions or compounds, and are easily segregated in the grain boundary in a spherical shape, which is one of the root causes of brittleness of steel at 200-480°C and cracks in welds. As an auxiliary material for steel smelting, the lead content of ferromolybdenum is required to be less than 0.1%, and the lead content for special users is required to be less than 0.05%.
[0003] my country's molybdenum resources are basically obtained from molybdenite in nature by flotation. Molybdenum mines are more or less associated with galena. Both molybdenite and galena have good flotation characteristics, which makes it inevitable that molybdenum concentrate contains lead. In the molybdenite treatment process with flotation as the main recovery method, it is very difficult to reduce the lead in molybdenum concentrate. At present, there are three commonly used methods: one is pre-control; the second is process control; the third is post-processing. Pre-control is to conduct a detailed survey of mine resources, select appropriate mining plans, reasonably allocate ores with different lead grades, control the lead content of the selected ore, and control the lead content in the ore from the source. Process control is to add galena inhibitors in the flotation process to inhibit the floating of galena, thereby reducing the lead content in the molybdenum concentrate. Post-processing is to use a wet method to reduce the content of impurities such as lead in molybdenum concentrate. The above methods have their own advantages and disadvantages. Pre-control is easy to achieve in large mines, but small mines have fewer mining sites and the ore is not easy to mix. Process control requires effective galena inhibitors. Common galena inhibitors include potassium dichromate, sodium cyanide, phospho(arsenic) Knox, sodium sulfide, etc., but potassium dichromate and sodium cyanide are highly toxic substances. my country has very strict control and it is very difficult to obtain them. Phospho(arsenic) Knox reagent is the product of the reaction between sodium hydroxide and phosphorus pentasulfide. It has a good lead inhibition effect in the molybdenum selection process, but it is easy to produce H2S, PH3 and a small amount of P2O5 during the configuration and use process, which are harmful to the human body and pose a great safety hazard. Post-processing generally uses chemical methods to remove trace lead in molybdenum concentrate, which reduces the molybdenum yield and is very costly. Summary of the invention
[0004] In order to solve the problems in the background technology, the present invention discloses a method for smelting and separating high-lead molybdenum concentrate. For high-lead molybdenum concentrate that is not effectively controlled or has relaxed control in the ore dressing process for various reasons, the lead volatilization characteristics of ferromolybdenum during high-temperature smelting are utilized to achieve molybdenum-lead separation in the smelting process. While ensuring that the ferromolybdenum product is qualified, the low-molybdenum and high-lead dust powder is further processed by alkali leaching for molybdenum-lead separation. This method can realize molybdenum-lead separation in the production process by combining smelting and selection with the lead content in the molybdenum concentrate that is difficult to control or reduce the standard in the molybdenum ore dressing process according to the characteristics of the ore source. The operation is simple and can be applied in industry.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0006] A method for smelting and separating high-lead molybdenum concentrate comprises the following steps:
[0007] Step 1: For high-lead molybdenum concentrate that is not effectively controlled or has been relaxed in the mineral processing process for various reasons, the high-lead molybdenum concentrate and the low-lead molybdenum concentrate are mixed and blended to control the lead content in the molybdenum concentrate to less than 1%, and the mixed molybdenum concentrate is oxidized and roasted to obtain high-lead molybdenum oxide. The oxidized roasting temperature of the molybdenum concentrate is 650°C, which is lower than the ignition point of lead sulfide. Lead continues to be enriched during the oxidized roasting process, but excessive lead agglomeration locally affects the roasting effect and the quality of molybdenum oxide;
[0008] Step 2: Mix the high-lead molybdenum oxide obtained in step 1 with auxiliary materials for smelting, adjust the auxiliary material ratio, increase the amount of aluminum particles and saltpeter, reduce the amount of ferrosilicon, ensure that the unit calorific value of the ferromolybdenum smelting reaction temperature is greater than 2300kJ / kg, ensure that the lead impurities are completely volatilized and enter the dust collecting powder, and smelt at a high temperature of 1600-2000°C to obtain a qualified ferromolybdenum product. The low-molybdenum and high-lead dust collecting powder generated during the smelting process is collected separately and not returned to the ferromolybdenum smelting furnace to ensure the quality of the ferromolybdenum product;
[0009] Step 3: using sodium sulfide or sodium sulfide + sodium hydroxide composite alkali leaching the low-molybdenum and high-lead dust collected in step 2, and separating the molybdenum-containing leaching solution and the leaching residue enriched with lead oxide after alkali leaching, and using the leaching residue as a low-grade lead concentrate for lead smelting;
[0010] Step 4: adjust the acidity of the molybdenum-containing leachate separated in step 3, preferably make the pH value of the sodium molybdate solution equal to 2-3, use weak alkaline macroporous ion exchange resin to enrich and remove impurities of molybdenum by ion exchange, and obtain post-handover liquid and negative molybdenum ion exchange resin respectively, use ammonia water to analyze the negative molybdenum ion exchange resin to obtain ammonium molybdate solution, and incorporate it into the molybdenum chemical system to produce ammonium molybdate, and the post-handover liquid is disposed of as wastewater.
[0011] Furthermore, in the method for smelting and separating high-lead molybdenum concentrate, the auxiliary materials for ferromolybdenum smelting in step 2 include ferrosilicon powder, aluminum particles, iron oxide scale, steel chips, calcium oxide and sodium nitrate.
[0012] Furthermore, in the method for smelting and separating high-lead molybdenum concentrate, the third alkali leaching adopts normal pressure leaching, the leaching temperature is 80-100°C, and the reaction time is 1-3h.
[0013] Furthermore, in the method for smelting and separating high-lead molybdenum concentrate, the solid ratio of the alkali leaching solution in step three is 2-5:1, and the amount of alkali used is 1.2-3 times the theoretical amount.
[0014] Furthermore, in the method for smelting and separating high-lead molybdenum concentrate, the alkaline leaching in step three adopts two countercurrent leachings, the molybdenum-containing leaching solution and the first leaching residue obtained by the first leaching separation are directly connected to step four, the second leaching solution and the low-grade lead concentrate obtained by the first leaching residue are again alkali-leached and separated, the second leaching solution is combined into the subsequent collection of high-lead dust powder for alkaline leaching, and the molybdenum content of the leaching residue is controlled to be less than 0.5% after two countercurrent washings.
[0015] Furthermore, in the method for smelting and separating high-lead molybdenum concentrate, the ion exchange resin in step four is D314 or D630 resin.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The method for smelting and separating high-lead molybdenum concentrate disclosed in the invention aims at high-lead molybdenum concentrate which cannot be effectively controlled or whose control is relaxed due to various reasons in the mineral processing link, realizes molybdenum-lead separation in the production process by combining mineral processing and smelting, controls the lead content to be less than 1% according to the lead content of the molybdenum concentrate, performs oxidative roasting, utilizes the lead volatilization characteristics of ferromolybdenum in high-temperature smelting to realize lead-molybdenum separation, and while ensuring that the quality of ferromolybdenum products meets the standards, collects low-molybdenum and high-lead dust powder separately and then realizes molybdenum-lead separation by alkali leaching, recovers the molybdenum-containing leachate and processes it in a molybdenum chemical production line to obtain an ammonium molybdate product, and the leached slag as a low-grade lead concentrate can be used as a primary raw material for lead smelting. The method is highly practical and easy to operate, and the laboratory test is consistent with the industrial test, and can be selectively adopted according to the high or low lead content of the molybdenum concentrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0019] Figure 1 It is a process flow chart of the method for smelting and separating high-lead molybdenum concentrate of the present invention. DETAILED DESCRIPTION
[0020] In order to better understand the present invention, the content of the present invention is further clearly set forth in conjunction with the embodiments below, but the protection content of the present invention is not limited to the following embodiments. In the following description, a large number of specific details are provided in order to provide a more thorough understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without one or more of these details.
[0021] Example 1 The molybdenum content of high-low lead molybdenum concentrates after mixing is 47.75%, and the lead content is 0.68%; the molybdenum content of molybdenum oxide after calcination in a converter at 650°C is 53.88%, and the lead content is 0.81%; the ingredients for ferromolybdenum smelting are as follows: 3800kg of molybdenum oxide, 915kg of ferrosilicon powder, 778kg of iron filings, 950kg of iron oxide, 440kg of aluminum particles, 270kg of calcium oxide, 50kg of saltpeter, and 550kg of crushed ferromolybdenum. After high-temperature smelting, the 60B ferromolybdenum product has a lead content of 0 .042%; the molybdenum content in the smelting dust powder is 7.48%, and the lead content is 34.59%. Take the smelting dust powder produced in Example 1, the single kettle feed amount is 150kg, and the dust powder is smelted by sodium sulfide alkaline leaching. The amount of sodium sulfide is twice the theoretical amount, the liquid-solid ratio is 4:1, the reaction temperature is 90-95℃, the reaction time is 2 hours, and the lead content in the leached residue after secondary countercurrent leaching and two countercurrent washings is 33.24%, and the molybdenum content is 0.45%. The leaching rates of lead and molybdenum are 1.24% and 96.77% respectively. The molybdenum-containing leaching solution is acidified to PH=2.5, and D314 or D630 anion exchange resin is used for adsorption. After ammonia solution is analyzed, purified, and acid precipitation is performed to obtain a first-grade ammonium molybdate product.
[0022] Example 2: After mixing, the molybdenum content of molybdenum concentrate is 47.83%, and the lead content is 0.78%; after converter roasting, the molybdenum content of molybdenum oxide is 54.52%, and the lead content is 0.89%; the ingredients for ferromolybdenum smelting are as follows: 4000kg of molybdenum oxide, 902kg of ferrosilicon powder, 744kg of iron filings, 1000kg of iron oxide, 516kg of aluminum particles, 260kg of calcium oxide, 70kg of saltpeter, and 400kg of crushed ferromolybdenum. After high-temperature smelting, 60A ferromolybdenum with a lead content of 0.036% is obtained; the molybdenum content of high-lead dust collection powder is 8. 25%, lead content 33.97%, take the smelting dust powder produced in Example 2, single kettle feed amount 150kg, use sodium hydroxide and sodium sulfide composite alkali alkali leaching to smelt dust powder, sodium hydroxide 40g / l, sodium sulfide is 1.2 times the theoretical amount of lead, liquid-solid ratio 4:1, reaction temperature 90-95℃, reaction time 2 hours, secondary countercurrent leaching, two countercurrent washings, the lead content in the leached slag is 36.24%, the molybdenum content is 0.42%, and the lead and molybdenum leaching rates of the first leaching are 1.52% and 96.75% respectively. The molybdenum-containing leaching solution is acidified to PH=2.5, D314 or D630 anion exchange resin is used for adsorption, and the first-grade ammonium molybdate product is obtained after ammonia solution analysis, purification, and acid precipitation.
[0023] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in the field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for smelting and separating high-lead molybdenum concentrate, characterized in that: The steps include: Step 1: Mix high-lead molybdenum concentrate and low-lead molybdenum concentrate to control the lead content in the molybdenum concentrate to less than 1%, and oxidize and roast the mixed molybdenum concentrate to obtain high-lead molybdenum oxide; Step 2: Mix the high-lead molybdenum oxide obtained in step 1 with auxiliary materials for smelting and then smelt ferromolybdenum to obtain ferromolybdenum product, and collect the high-lead dust powder generated during the smelting process separately; Step 3: using sodium sulfide or sodium sulfide + sodium hydroxide composite alkali to alkali-leach the high-lead dust powder collected in step 2, and separating the molybdenum-containing leaching solution and the leaching residue enriched with lead oxide after alkali leaching, and the leaching residue is used for lead smelting; Step 4: After the molybdenum-containing leachate separated in step 3 is acidified, a weakly alkaline macroporous ion exchange resin is used to adsorb molybdenum through ion exchange to obtain a post-handling liquid and a negative molybdenum ion exchange resin. The negative molybdenum ion exchange resin is decomposed with ammonia water to obtain an ammonium molybdate solution, which is incorporated into the molybdenum chemical system to produce ammonium molybdate, and the post-handling liquid is disposed of as wastewater.
2. The method for smelting and separating high-lead molybdenum concentrate according to claim 1, characterized in that: The unit calorific value of the reaction temperature of molybdenum iron smelting in step 2 is greater than 2300 kJ / kg.
3. The method for smelting and separating high-lead molybdenum concentrate according to claim 1, characterized in that: Step 2: Ferromolybdenum smelting: Auxiliary materials for smelting include ferrosilicon powder, aluminum particles, iron oxide scale, steel chips, calcium oxide and sodium nitrate.
4. The method for smelting and separating high-lead molybdenum concentrate according to claim 1, characterized in that: In step three, alkaline leaching is performed at normal pressure, with a leaching temperature of 80-100° C. and a reaction time of 1-3 hours.
5. The method for smelting and separating high-lead molybdenum concentrate according to claim 1, characterized in that: In step three, the solid ratio of the alkali leaching solution is equal to 2-5:1, and the amount of alkali used is 1.2-3 times the theoretical amount.
6. The method for smelting and separating high-lead molybdenum concentrate according to claim 1, characterized in that: In step three, alkaline leaching adopts two countercurrent leachings. The molybdenum-containing leaching solution and the first leaching residue obtained by the first leaching separation are directly connected to step four. The second leaching solution and the low-grade lead concentrate obtained by the first leaching residue are separated by alkaline leaching again. The second leaching solution is combined into the subsequent collection of high-lead dust powder for alkaline leaching.
7. The method for smelting and separating high-lead molybdenum concentrate according to claim 1, characterized in that: In step 4, the ion exchange resin is D314 or D630 resin.