A method for preparing flame-retardant polyester fiber

Through the melt blending technology of modified ammonium polyphosphate and polyester powder, the problems of flammability and poor compatibility of polyester fibers are solved, and the preparation of flame retardant polyester fibers with both flame retardant properties and mechanical properties is achieved. Achieved UL-94 V0 flame retardant grade and high fracture strength.

CN118516780BActive Publication Date: 2024-11-19JIANGSU HENGLI CHEM FIBER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985882.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-19
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Polyester fibers are flammable and have severe melting droplets during combustion, and have insufficient flame retardant performance. Especially in areas with high flame retardant performance requirements, there are application restrictions. The poor compatibility of existing modified ammonium polyphosphate and polyester leads to mechanical properties. Serious losses.

Method used

Modified ammonium polyphosphate flame retardant is used to react with a mixed solution of hydroxybenzaldehyde, aniline and dicyandiamide in ethanol and water to form a covalent bond graft structure, and after modification, it is melted and co-existed with the polyester powder. Blend wire to prepare flame retardant polyester fibers to improve their compatibility and flame retardant properties.

Benefits of technology

It has achieved high-efficiency flame retardant properties of flame retardant polyester fibers, with a fracture strength of no less than 3.1cN/dtex, an ultimate oxygen index of 29.8~32.5%. There is no melt droplet generated in the UL-94 vertical combustion test, and the flame retardant level reaches V0. Minor damage to mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118516780B_ABST
    Figure CN118516780B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a flame-retardant polyester fiber, wherein the flame-retardant polyester masterbatch and polyester chips are melt-blended and spun to obtain the flame-retardant polyester fiber; the flame-retardant polyester masterbatch is obtained by mixing a modified ammonium polyphosphate flame retardant with polyester powder and then putting the mixture into a twin-screw extruder for melt blending and extrusion granulation in sequence; the preparation method of the modified ammonium polyphosphate flame retardant is as follows: ammonium polyphosphate, hydroxybenzaldehyde, aniline and dicyandiamide are added to a mixed solution of ethanol and water and uniformly dispersed, stirred and reacted at 65-75°C, and after the reaction, reduced pressure distillation is performed until 1 / 4-1 / 3 of the mixed solution of ethanol and water remains, and then the product is sequentially dried, washed and dried to obtain the modified ammonium polyphosphate flame retardant. The modified ammonium polyphosphate flame retardant of the present invention has good compatibility with polyester fiber, excellent flame retardant performance of the flame-retardant polyester fiber, and less damage to the mechanical properties of the polyester fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame-retardant polyester fibers and relates to a method for preparing the flame-retardant polyester fibers. Background Art

[0002] Polyester fiber is the most produced and widely used synthetic fiber with excellent dimensional stability and chemical resistance. However, polyester fiber is flammable and has severe droplets when burning, which seriously limits its application in fields with special requirements for flame retardant properties.

[0003] In order to improve the flame retardant properties of polyester fibers, researchers often use the method of adding flame retardants. Among them, ammonium polyphosphate is a highly efficient halogen-free flame retardant with high phosphorus and nitrogen content, good flame retardant effect, and high decomposition temperature. However, ammonium polyphosphate has poor compatibility with polyester, and the addition of blends has a significant impact on the mechanical properties of polyester fibers.

[0004] In response to the above problems, it is of great significance to modify ammonium polyphosphate to improve its interfacial compatibility with polyester and ensure that its flame retardant properties are improved without affecting the mechanical properties of the material, but there are great challenges.

[0005] For example, Reference 1 (Preparation of inorganic-organic composite modified ammonium polyphosphate and its application in unsaturated polyester [J]. Plastic Industry, 2015, 43(7): 97-101.) used silica and silane coupling agent KH570 to modify the surface of ammonium polyphosphate to obtain an inorganic-organic composite modified ammonium polyphosphate and prepared ammonium polyphosphate / unsaturated polyester (UP) composite materials. However, the compatibility between KH570 and polyester is still poor, especially for fibrous composite materials, the loss of mechanical properties is particularly serious.

[0006] Reference 2 (Effect of hyperbranched polysiloxane-coated ammonium polyphosphate on the flame retardant properties of PET [J]. Industrial Textiles, 2021, 39(4): 12-19.) Ammonium polyphosphate was modified by hyperbranched polysiloxane to synthesize a hyperbranched polysiloxane-coated ammonium polyphosphate intumescent flame retardant, and a flame-retardant poly composite material was prepared by melt blending technology. However, the compatibility between hyperbranched polysiloxane and polyester is still poor, which seriously damages the mechanical properties of the polyester material.

[0007] Therefore, it is of great significance to study a method for preparing flame retardant polyester fiber to solve the problems existing in the prior art. Summary of the invention

[0008] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for preparing flame retardant polyester fiber.

[0009] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing flame-retardant polyester fiber, wherein flame-retardant polyester masterbatch and polyester chips are melt-blended and spun to obtain flame-retardant polyester fiber;

[0011] The flame retardant polyester masterbatch is obtained by mixing the modified ammonium polyphosphate flame retardant with polyester powder and then feeding the mixture into a twin-screw extruder for melt blending and extrusion granulation.

[0012] The preparation method of the modified ammonium polyphosphate flame retardant is as follows: adding ammonium polyphosphate, hydroxybenzaldehyde, aniline and dicyandiamide into a mixed solution of ethanol and water and uniformly dispersing them, stirring and reacting them at 65-75°C, hydroxybenzaldehyde being easily soluble in ethanol and hot water, and the increase of the reaction temperature is helpful to improve the molecular movement and promote the modification of ammonium polyphosphate by hydroxybenzaldehyde and aniline, performing reduced pressure distillation after the reaction until 1 / 4-1 / 3 of the mixed solution of ethanol and water remains, and then drying, washing and drying the product in sequence to obtain the modified ammonium polyphosphate flame retardant;

[0013] The hydroxybenzaldehyde is one or more of 4,5-trihydroxybenzaldehyde, p-hydroxybenzaldehyde and 2,5-dihydroxyterephthalaldehyde;

[0014] Dicyandiamide is a catalyst that helps promote the covalent bond grafting reaction between the ammonium phosphate structure of ammonium polyphosphate and the hydroxyl group of hydroxybenzaldehyde;

[0015] Distilling under reduced pressure until only 1 / 4 to 1 / 3 of the solvent (mixed solution of ethanol and water) remains helps create a humid environment and promotes the reaction between ammonium polyphosphate and hydroxybenzaldehyde in the subsequent high-temperature drying process.

[0016] As the preferred technical solution:

[0017] In the method for preparing a flame retardant polyester fiber as described above, the amount of the flame retardant polyester masterbatch is 10-15% based on the total mass of the flame retardant polyester masterbatch and the polyester chips.

[0018] In the method for preparing a flame-retardant polyester fiber as described above, the flame-retardant polyester masterbatch and the polyester chips are respectively subjected to pre-crystallization and drying treatment before melt blending and spinning, so as to ensure that the final moisture of the flame-retardant polyester masterbatch and the polyester chips is less than 100 ppm;

[0019] The pre-crystallization temperature of flame-retardant polyester masterbatch is 90~110℃, the pre-crystallization time is 3~4h, the drying temperature is 120~140℃, and the drying time is 10~15h;

[0020] The pre-crystallization temperature of polyester chips is 90~110℃, the pre-crystallization time is 3~4h, the drying temperature is 120~140℃, and the drying time is 10~15h.

[0021] In the method for preparing a flame-retardant polyester fiber as described above, the process parameters of melt blending spinning are: spinning temperature 260-270°C, spinning speed 1500-2000 m / min, and draft ratio 1.5-3.

[0022] In the method for preparing a flame-retardant polyester fiber as described above, based on the total mass of the modified ammonium polyphosphate flame retardant and the polyester powder, the amount of the modified ammonium polyphosphate flame retardant is 20-25%.

[0023] In the method for preparing a flame-retardant polyester fiber as described above, the modified ammonium polyphosphate flame retardant and the polyester powder are dried separately before melt blending;

[0024] The drying temperature of modified ammonium polyphosphate flame retardant is 60~80℃, and the drying time is 7~9h;

[0025] The drying temperature of polyester powder is 120~130℃, and the drying time is 10~12h.

[0026] In the method for preparing a flame-retardant polyester fiber as described above, the processing temperature of the twin-screw extruder is 250-260°C, and the processing speed is 20-25r / min; if the processing temperature is too low, the modified ammonium polyphosphate flame retardant and the polyester powder cannot be mixed evenly, which is not conducive to granulation, and if the temperature is too high, it will cause energy waste. In the temperature range of 250-260°C of the present invention, uniform flame-retardant polyester masterbatch can be successfully prepared.

[0027] In the method for preparing a flame-retardant polyester fiber as described above, ammonium polyphosphate is a type II flame retardant, and the degree of polymerization of ammonium polyphosphate is greater than 1000.

[0028] In the method for preparing a flame-retardant polyester fiber as described above, the mass ratio of hydroxybenzaldehyde to ammonium polyphosphate is 1-2:5, the molar ratio of aniline to hydroxybenzaldehyde is 1.3-1.5:1, the higher the amount of hydroxybenzaldehyde used, the more helpful it is to modify the ammonium polyphosphate, but too high an amount is wasteful; theoretically, one mole of aniline can react with one mole of hydroxybenzaldehyde to produce a Schiff base reaction, and excess aniline helps promote the reaction, but too high an amount is wasteful; the mass ratio of dicyandiamide to ammonium polyphosphate is 1-2:10, the amount ratio of ammonium polyphosphate to a mixed solution of ethanol and water is 1 g:3-5 mL, and the volume proportion of ethanol in the mixed solution of ethanol and water is 50-70%.

[0029] In the method for preparing a flame-retardant polyester fiber as described above, the stirring reaction time is 60 to 90 minutes;

[0030] The pressure of vacuum distillation is 35~45kPa and the temperature is 40~50℃;

[0031] The drying temperature is 160~170℃. A higher drying temperature is helpful to promote the esterification reaction between ammonium polyphosphate and hydroxybenzaldehyde. The drying time is 30~60min.

[0032] Washing refers to washing with distilled water and ethanol respectively;

[0033] The drying temperature is 70~90℃ and the time is 30~50min.

[0034] A method for preparing a flame-retardant polyester fiber as described above, the flame-retardant polyester fiber has a breaking strength of not less than 3.1 cN / dtex, a limiting oxygen index of 29.8~32.5%, a flame retardancy grade of V0 in a UL-94 vertical burning test, and no droplets are generated in a UL-94 vertical burning test (the breaking strength of the polyester fiber that has not been flame-retardantly modified is 3.4 cN / dtex, the limiting oxygen index is 20.1%, droplets are generated in a UL-94 vertical burning test, the flame retardancy grade is NR, the droplets are serious, and the flame retardancy is poor).

[0035] The principle of the present invention is:

[0036] Ammonium polyphosphate contains high phosphorus and nitrogen contents in its structure and has high flame retardant efficiency; however, ammonium polyphosphate has poor compatibility with polyester fibers and cannot be evenly dispersed in polyester fibers, resulting in poor flame retardant efficiency of ammonium polyphosphate-modified polyester fibers and serious loss of mechanical properties.

[0037] The ammonium polyphosphate structure is rich in ammonium phosphate structures, which can undergo esterification cross-linking reactions with the hydroxyl groups of hydroxybenzaldehyde, so that the hydroxybenzaldehyde can be stably coated on the surface of the ammonium polyphosphate particles through covalent bonds, thereby achieving surface modification of the ammonium polyphosphate; at the same time, the amino groups of aniline can undergo Schiff base reactions with the aldehyde groups of hydroxybenzaldehyde, thereby further introducing benzene rings for modification. After modification, the benzene ring structure can be evenly covered on the surface of the ammonium polyphosphate through covalent bonding. The surface of the modified ammonium polyphosphate is rich in benzene ring structures, which coat the ammonium polyphosphate inside, and the ammonium polyphosphate does not directly contact the polyester. Therefore, the modified ammonium polyphosphate flame retardant has high compatibility with polyester, can be well dispersed in polyester fibers, is not easy to migrate and precipitate, and has little damage to the mechanical properties of the flame-retardant polyester fibers.

[0038] Ammonium polyphosphate is rich in phosphate and can act as an acid source. Its ammonium and Schiff base structures act as gas sources. The hydroxyl groups containing hydroxybenzaldehyde act as aromatic carbon formers. Various structures are organically combined to form an intumescent flame retardant system. The introduction of Schiff base structure also helps to improve the thermal stability of flame retardant polyester fibers. Modified ammonium polyphosphate flame retardant can produce intumescent carbon residue during combustion, which effectively improves the flame retardant properties of polyester fibers.

[0039] Beneficial effects:

[0040] (1) A method for preparing a flame-retardant polyester fiber of the present invention comprises modifying ammonium polyphosphate with hydroxybenzaldehyde and aniline under the catalysis of dicyandiamide, wherein the modified ammonium polyphosphate flame retardant has good compatibility with the polyester fiber, the flame-retardant polyester fiber has excellent flame retardant properties, and has little damage to the mechanical properties of the polyester fiber;

[0041] (2) In the method for preparing a flame-retardant polyester fiber of the present invention, the modified ammonium polyphosphate flame retardant can produce expanded carbon residue during combustion, thereby effectively improving the flame retardant properties of the polyester fiber. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The schematic diagram of the structure of the modified ammonium polyphosphate flame retardant containing 4,5-trihydroxybenzaldehyde as the hydroxybenzaldehyde of the present invention. DETAILED DESCRIPTION

[0043] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0044] The test methods involved in the performance indicators in the embodiments and comparative examples of the present invention are as follows:

[0045] Breaking strength: Tested in accordance with GB / T 14344-2022 "Test method for tensile properties of chemical fiber filaments";

[0046] Limiting oxygen index: Tested in accordance with FZ / T 50017-2011 "Test method for flame retardancy of polyester fibers - oxygen index method".

[0047] The polyester powder and polyester chips of the present invention are from Yizheng Chemical Fiber, with the trade name FG650; the ammonium polyphosphate is from McLean, with the trade name A875132.

[0048] Example 1

[0049] A method for preparing a flame retardant polyester fiber, the specific steps are as follows:

[0050] (1) Add ammonium polyphosphate, 2,5-dihydroxyterephthalaldehyde, aniline and dicyandiamide to a mixed solution of ethanol and water and disperse them uniformly. Stir and react at 70°C for 75 minutes. After the reaction, vacuum distillation is performed at a pressure of 45 kPa and a temperature of 50°C until the mixed solution of ethanol and water remains 1 / 4. The product is then dried at 165°C for 45 minutes, washed with distilled water and ethanol respectively, and finally dried at 90°C for 30 minutes to obtain a structure as shown in Figure 1 The modified ammonium polyphosphate flame retardant shown;

[0051] The mass ratio of 2,5-dihydroxyterephthalaldehyde to ammonium polyphosphate is 1.5:5, the molar ratio of aniline to 2,5-dihydroxyterephthalaldehyde is 1.5:1, the mass ratio of dicyandiamide to ammonium polyphosphate is 1.5:10, the dosage ratio of ammonium polyphosphate to the mixed solution of ethanol and water is 1 g:4 mL, and the volume proportion of ethanol in the mixed solution of ethanol and water is 60%;

[0052] (2) The modified ammonium polyphosphate flame retardant was dried at 80°C for 7 hours, and the polyester powder was dried at 130°C for 10 hours;

[0053] (3) mixing the dried modified ammonium polyphosphate flame retardant with polyester powder and feeding the mixture into a twin-screw extruder to perform melt blending and extrusion granulation to obtain a flame-retardant polyester masterbatch;

[0054] Among them, the processing temperature of the twin-screw extruder is 260°C and the processing speed is 25r / min;

[0055] Based on the total mass of modified ammonium polyphosphate flame retardant and polyester powder, the amount of modified ammonium polyphosphate flame retardant is 23%;

[0056] (4) The flame retardant polyester masterbatch was pre-crystallized at 100°C for 3.5 hours and then dried at 130°C for 13 hours;

[0057] (5) The polyester chips were pre-crystallized at 100°C for 3.5 hours and then dried at 130°C for 13 hours;

[0058] (6) melt-blending and spinning the flame-retardant polyester masterbatch treated in step (4) and the polyester chips treated in step (5) to produce flame-retardant polyester fibers;

[0059] Among them, based on the total mass of flame retardant polyester masterbatch and polyester chips, the amount of flame retardant polyester masterbatch is 13%;

[0060] The process parameters of melt blending spinning are: spinning temperature 270°C, spinning speed 1700m / min, and draft ratio 2.

[0061] The final flame-retardant polyester fiber has a breaking strength of 3.2 cN / dtex, a limiting oxygen index of 31.7%, a flame retardancy grade of V0 in the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test.

[0062] Comparative Example 1

[0063] A method for preparing a flame-retardant polyester fiber is basically the same as that of Example 1, except that the hydroxybenzaldehyde is omitted in step (1).

[0064] The final flame-retardant polyester fiber has a breaking strength of 2.3 cN / dtex, a limiting oxygen index of 27.3%, a flame retardancy grade of V1 in the UL-94 vertical burning test, and 5 droplets are generated in the UL-94 vertical burning test.

[0065] By comparing Comparative Example 1 with Example 1, it can be found that the flame retardant properties of the ammonium polyphosphate flame-retardant polyester fiber that has not been modified with hydroxybenzaldehyde are reduced, and the breaking strength is reduced. This is because aniline alone cannot modify the ammonium polyphosphate, resulting in reduced dispersion of the ammonium polyphosphate flame retardant in the polyester fiber, reduced flame retardant efficiency, and serious loss of mechanical properties.

[0066] Comparative Example 2

[0067] A method for preparing a flame-retardant polyester fiber is basically the same as that of Example 1, except that aniline is omitted in step (1).

[0068] The final flame-retardant polyester fiber has a breaking strength of 2.6 cN / dtex, a limiting oxygen index of 28.5%, and a flame retardancy grade of V0 in a UL-94 vertical burning test.

[0069] By comparing Comparative Example 1 with Example 1, it can be found that the flame retardant properties of the ammonium polyphosphate flame-retardant polyester fiber that is not modified with aniline are reduced, and the breaking strength is reduced. This is because the ammonium polyphosphate flame retardant modified with hydroxybenzaldehyde alone has a limited amount of hydroxybenzaldehyde grafted on the ammonium polyphosphate due to the steric hindrance effect, which makes the dispersion performance of the ammonium polyphosphate flame retardant modified with hydroxybenzaldehyde in the polyester fiber still poor, the flame retardant efficiency is reduced, and the mechanical properties are seriously lost.

[0070] Example 2

[0071] A method for preparing a flame retardant polyester fiber, the specific steps are as follows:

[0072] (1) Add ammonium polyphosphate, p-hydroxybenzaldehyde, aniline and dicyandiamide to a mixed solution of ethanol and water and uniformly disperse them, stir and react at 68°C for 80 minutes, and after the reaction, perform vacuum distillation at a pressure of 40 kPa and a temperature of 45°C until the mixed solution of ethanol and water remains 1 / 3, then dry the product at 162°C for 50 minutes, wash with distilled water and ethanol respectively, and finally dry at 80°C for 40 minutes to obtain a modified ammonium polyphosphate flame retardant;

[0073] Among them, the mass ratio of p-hydroxybenzaldehyde to ammonium polyphosphate is 1.3:5, the molar ratio of aniline to p-hydroxybenzaldehyde is 1.4:1, the mass ratio of dicyandiamide to ammonium polyphosphate is 1.3:10, the dosage ratio of ammonium polyphosphate to the mixed solution of ethanol and water is 1g:3.5mL, and the volume proportion of ethanol in the mixed solution of ethanol and water is 55%;

[0074] (2) The modified ammonium polyphosphate flame retardant was dried at 70°C for 8 hours, and the polyester powder was dried at 125°C for 11 hours;

[0075] (3) mixing the dried modified ammonium polyphosphate flame retardant with polyester powder and feeding the mixture into a twin-screw extruder to perform melt blending and extrusion granulation to obtain a flame-retardant polyester masterbatch;

[0076] Among them, the processing temperature of the twin-screw extruder is 255°C and the processing speed is 23r / min;

[0077] Based on the total mass of modified ammonium polyphosphate flame retardant and polyester powder, the amount of modified ammonium polyphosphate flame retardant is 21%;

[0078] (4) The flame retardant polyester masterbatch was pre-crystallized at 95°C for 3.7 hours and then dried at 125°C for 14 hours;

[0079] (5) The polyester chips were pre-crystallized at 95°C for 3.7 hours and then dried at 125°C for 14 hours;

[0080] (6) melt-blending and spinning the flame-retardant polyester masterbatch treated in step (4) and the polyester chips treated in step (5) to produce flame-retardant polyester fibers;

[0081] Among them, based on the total mass of flame retardant polyester masterbatch and polyester chips, the amount of flame retardant polyester masterbatch is 11%;

[0082] The process parameters of melt blending spinning are: spinning temperature 265°C, spinning speed 1600m / min, and draft ratio 2.

[0083] The final flame-retardant polyester fiber has a breaking strength of 3.2 cN / dtex, a limiting oxygen index of 30.9%, a flame retardancy grade of V0 in the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test.

[0084] Example 3

[0085] A method for preparing a flame retardant polyester fiber, the specific steps are as follows:

[0086] (1) adding ammonium polyphosphate, 4,5-trihydroxybenzaldehyde, aniline and dicyandiamide to a mixed solution of ethanol and water and uniformly dispersing them, stirring and reacting them at 65°C for 90 minutes, and after the reaction, performing reduced pressure distillation at a pressure of 35 kPa and a temperature of 40°C until the mixed solution of ethanol and water remains 1 / 4, and then drying the product at 160°C for 60 minutes, washing with distilled water and ethanol respectively, and finally drying at 70°C for 50 minutes to obtain a modified ammonium polyphosphate flame retardant;

[0087] The mass ratio of 4,5-trihydroxybenzaldehyde to ammonium polyphosphate is 1:5, the molar ratio of aniline to 4,5-trihydroxybenzaldehyde is 1.3:1, the mass ratio of dicyandiamide to ammonium polyphosphate is 1:10, the dosage ratio of ammonium polyphosphate to the mixed solution of ethanol and water is 1 g:3 mL, and the volume proportion of ethanol in the mixed solution of ethanol and water is 50%;

[0088] (2) drying the modified ammonium polyphosphate flame retardant at 60°C for 9 hours, and drying the polyester powder at 120°C for 12 hours;

[0089] (3) mixing the dried modified ammonium polyphosphate flame retardant with polyester powder and feeding the mixture into a twin-screw extruder to perform melt blending and extrusion granulation to obtain a flame-retardant polyester masterbatch;

[0090] Among them, the processing temperature of the twin-screw extruder is 250°C and the processing speed is 20r / min;

[0091] Based on the total mass of modified ammonium polyphosphate flame retardant and polyester powder, the amount of modified ammonium polyphosphate flame retardant is 20%;

[0092] (4) The flame retardant polyester masterbatch was pre-crystallized at 90°C for 4 hours and then dried at 120°C for 15 hours;

[0093] (5) The polyester chips were pre-crystallized at 90°C for 4 hours and then dried at 120°C for 15 hours;

[0094] (6) melt-blending and spinning the flame-retardant polyester masterbatch treated in step (4) and the polyester chips treated in step (5) to produce flame-retardant polyester fibers;

[0095] Among them, based on the total mass of flame retardant polyester masterbatch and polyester chips, the amount of flame retardant polyester masterbatch is 10%;

[0096] The process parameters of melt blending spinning are: spinning temperature 260°C, spinning speed 1500m / min, and draft ratio 2.

[0097] The final flame-retardant polyester fiber has a breaking strength of 3.3 cN / dtex, a limiting oxygen index of 29.8%, a flame retardancy grade of V0 in the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test.

[0098] Example 4

[0099] A method for preparing a flame retardant polyester fiber, the specific steps are as follows:

[0100] (1) adding ammonium polyphosphate, 4,5-trihydroxybenzaldehyde, aniline and dicyandiamide to a mixed solution of ethanol and water and uniformly dispersing them, stirring and reacting them at 72°C for 70 minutes, and after the reaction, performing reduced pressure distillation at a pressure of 40 kPa and a temperature of 45°C until the mixed solution of ethanol and water remains 1 / 3, and then drying the product at 168°C for 40 minutes, washing with distilled water and ethanol respectively, and finally drying at 75°C for 45 minutes to obtain a modified ammonium polyphosphate flame retardant;

[0101] The mass ratio of 4,5-trihydroxybenzaldehyde to ammonium polyphosphate is 1.8:5, the molar ratio of aniline to 4,5-trihydroxybenzaldehyde is 1.4:1, the mass ratio of dicyandiamide to ammonium polyphosphate is 1.8:10, the dosage ratio of ammonium polyphosphate to the mixed solution of ethanol and water is 1 g:4.5 mL, and the volume proportion of ethanol in the mixed solution of ethanol and water is 65%;

[0102] (2) The modified ammonium polyphosphate flame retardant was dried at 80°C for 7 hours, and the polyester powder was dried at 130°C for 10 hours;

[0103] (3) mixing the dried modified ammonium polyphosphate flame retardant with polyester powder and feeding the mixture into a twin-screw extruder to perform melt blending and extrusion granulation to obtain a flame-retardant polyester masterbatch;

[0104] Among them, the processing temperature of the twin-screw extruder is 255°C and the processing speed is 22r / min;

[0105] Based on the total mass of modified ammonium polyphosphate flame retardant and polyester powder, the amount of modified ammonium polyphosphate flame retardant is 24%;

[0106] (4) The flame retardant polyester masterbatch was pre-crystallized at 105°C for 3.3 hours and then dried at 135°C for 12 hours;

[0107] (5) The polyester chips were pre-crystallized at 105°C for 3.3 hours and then dried at 135°C for 12 hours;

[0108] (6) melt-blending and spinning the flame-retardant polyester masterbatch treated in step (4) and the polyester chips treated in step (5) to produce flame-retardant polyester fibers;

[0109] Among them, based on the total mass of flame retardant polyester masterbatch and polyester chips, the amount of flame retardant polyester masterbatch is 14%;

[0110] The process parameters of melt blending spinning are: spinning temperature 265°C, spinning speed 1900m / min, and draft ratio 2.

[0111] The final flame-retardant polyester fiber has a breaking strength of 3.1 cN / dtex, a limiting oxygen index of 31.8%, a flame retardancy grade of V0 in the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test.

[0112] Example 5

[0113] A method for preparing a flame retardant polyester fiber, the specific steps are as follows:

[0114] (1) adding ammonium polyphosphate, a mixture of p-hydroxybenzaldehyde and 2,5-dihydroxyterephthalaldehyde in a mass ratio of 1:1, aniline and dicyandiamide to a mixed solution of ethanol and water and uniformly dispersing them, stirring and reacting them at 75°C for 60 minutes, and after the reaction, performing reduced pressure distillation at a pressure of 35 kPa and a temperature of 40°C until the mixed solution of ethanol and water remains 1 / 4, and then drying the product at 170°C for 30 minutes, washing with distilled water and ethanol respectively, and finally drying at 85°C for 35 minutes to obtain a modified ammonium polyphosphate flame retardant;

[0115] The mass ratio of the mixture of p-hydroxybenzaldehyde and 2,5-dihydroxyterephthalaldehyde in a mass ratio of 1:1 to ammonium polyphosphate is 2:5, the molar ratio of aniline to the mixture of p-hydroxybenzaldehyde and 2,5-dihydroxyterephthalaldehyde in a mass ratio of 1:1 is 1.5:1, the mass ratio of dicyandiamide to ammonium polyphosphate is 2:10, the amount ratio of ammonium polyphosphate to the mixed solution of ethanol and water is 1 g:5 mL, and the volume proportion of ethanol in the mixed solution of ethanol and water is 70%;

[0116] (2) drying the modified ammonium polyphosphate flame retardant at 60°C for 9 hours, and drying the polyester powder at 120°C for 12 hours;

[0117] (3) mixing the dried modified ammonium polyphosphate flame retardant with polyester powder and feeding the mixture into a twin-screw extruder to perform melt blending and extrusion granulation to obtain a flame-retardant polyester masterbatch;

[0118] Among them, the processing temperature of the twin-screw extruder is 250°C and the processing speed is 20r / min;

[0119] Based on the total mass of modified ammonium polyphosphate flame retardant and polyester powder, the amount of modified ammonium polyphosphate flame retardant is 25%;

[0120] (4) The flame retardant polyester masterbatch was pre-crystallized at 110°C for 3 hours and then dried at 140°C for 10 hours;

[0121] (5) The polyester chips were pre-crystallized at 110°C for 3 hours and then dried at 140°C for 10 hours;

[0122] (6) melt-blending and spinning the flame-retardant polyester masterbatch treated in step (4) and the polyester chips treated in step (5) to produce flame-retardant polyester fibers;

[0123] Among them, based on the total mass of flame retardant polyester masterbatch and polyester chips, the amount of flame retardant polyester masterbatch is 15%;

[0124] The process parameters of melt blending spinning are: spinning temperature 260°C, spinning speed 2000m / min, and draft ratio 2.

[0125] The final flame-retardant polyester fiber has a breaking strength of 3.1 cN / dtex, a limiting oxygen index of 32.5%, a flame retardancy grade of V0 in the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test.

Claims

1. A method for preparing a flame retardant polyester fiber, characterized in that: The flame retardant polyester masterbatch and polyester chips are melt blended and spun to obtain flame retardant polyester fibers; The flame retardant polyester masterbatch is obtained by mixing the modified ammonium polyphosphate flame retardant with polyester powder and then feeding the mixture into a twin-screw extruder for melt blending and extrusion granulation. The preparation method of the modified ammonium polyphosphate flame retardant is as follows: adding ammonium polyphosphate, hydroxybenzaldehyde, aniline and dicyandiamide into a mixed solution of ethanol and water and uniformly dispersing them, stirring and reacting them at 65-75°C, performing reduced pressure distillation after the reaction until 1 / 4-1 / 3 of the mixed solution of ethanol and water remains, and then drying, washing and drying the product in sequence to obtain the modified ammonium polyphosphate flame retardant; The mass ratio of hydroxybenzaldehyde to ammonium polyphosphate is 1-2:5, the molar ratio of aniline to hydroxybenzaldehyde is 1.3-1.5:1, the mass ratio of dicyandiamide to ammonium polyphosphate is 1-2:10, the dosage ratio of ammonium polyphosphate to a mixed solution of ethanol and water is 1 g:3-5 mL, and the volume proportion of ethanol in the mixed solution of ethanol and water is 50-70%.

2. The method for preparing a flame-retardant polyester fiber according to claim 1, characterized in that: Based on the total mass of flame retardant polyester masterbatch and polyester chips, the dosage of flame retardant polyester masterbatch is 10~15%.

3. The method for preparing a flame-retardant polyester fiber according to claim 1, characterized in that: The flame retardant polyester masterbatch and polyester chips are pre-crystallized and dried before melt blending and spinning; The pre-crystallization temperature of flame-retardant polyester masterbatch is 90~110℃, the pre-crystallization time is 3~4h, the drying temperature is 120~140℃, and the drying time is 10~15h; The pre-crystallization temperature of polyester chips is 90~110℃, the pre-crystallization time is 3~4h, the drying temperature is 120~140℃, and the drying time is 10~15h.

4. The method for preparing a flame-retardant polyester fiber according to claim 1, characterized in that: The process parameters of melt blending spinning are: spinning temperature 260~270℃, spinning speed 1500~2000m / min, and draft ratio 1.5~3.

5. The method for preparing a flame-retardant polyester fiber according to claim 1, characterized in that: Based on the total mass of the modified ammonium polyphosphate flame retardant and the polyester powder, the dosage of the modified ammonium polyphosphate flame retardant is 20-25%.

6. The method for preparing a flame retardant polyester fiber according to claim 1, characterized in that: The modified ammonium polyphosphate flame retardant and the polyester powder are dried separately before melt blending; The drying temperature of modified ammonium polyphosphate flame retardant is 60~80℃, and the drying time is 7~9h; The drying temperature of polyester powder is 120~130℃, and the drying time is 10~12h.

7. The method for preparing a flame-retardant polyester fiber according to claim 1, characterized in that: The processing temperature of the twin-screw extruder is 250~260℃, and the processing speed is 20~25r / min.

8. The method for preparing a flame-retardant polyester fiber according to claim 1, characterized in that: The degree of polymerization of ammonium polyphosphate is greater than 1000.

9. The method for preparing a flame-retardant polyester fiber according to claim 1, characterized in that: The stirring reaction time is 60~90min; The pressure of vacuum distillation is 35~45kPa and the temperature is 40~50℃; The drying temperature is 160~170℃ and the time is 30~60min; Washing refers to washing with distilled water and ethanol respectively; The drying temperature is 70~90℃ and the time is 30~50min.

10. The method for preparing a flame retardant polyester fiber according to claim 1, characterized in that: The breaking strength of the flame-retardant polyester fiber is not less than 3.1 cN / dtex, the limiting oxygen index is 29.8~32.5%, the flame retardancy level of the UL-94 vertical burning test is V0, and no molten droplets are generated in the UL-94 vertical burning test.