Long fiber needle punching preparation method of carbon fiber felt for vanadium redox flow battery VRFB

Through cross-laying, needle puncture and chemical modification, the structural and surface characteristics of carbon fiber felt are optimized, and the problems of weak interlayer strength and complex process in the prior art are solved, which significantly improves the stretching and interlayer of carbon fiber felt. The shear strength meets the high performance needs of vanadium redox flow batteries.

CN118516809BActive Publication Date: 2024-11-12烟台奥森制动材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410969535.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-12
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

The existing carbon fiber needle puncture process has the disadvantages of weak interlayer strength, complex process, long cycle and high cost, and it is difficult to meet the high-performance material needs of vanadium redox flow battery VRFB.

Method used

The structural and surface characteristics of carbon fiber felt are optimized by cross-laying, one-way laminated needle puncture, multi-stage needle puncture, edge cutting and winding and chemical modification. The mechanical strength is enhanced by cross-laying, and the one-way laminated needle is enhanced. Puncture improves material integrity, multi-stage needle puncture adjusts pore structure, chemical modification improves electrochemical performance, and finally improves tensile strength and interlayer shear strength through organic strontium modification liquid and hydrogen peroxide treatment.

Benefits of technology

It significantly improves the tensile strength and interlayer shear strength of carbon fiber felt, improves the mechanical and electrochemical properties of the material, and meets the high surface area and low resistance requirements of vanadium redox flow batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of long fiber needle punching of carbon fiber felt, and discloses a long fiber needle punching preparation method of carbon fiber felt for vanadium redox flow battery VRFB. The method comprises: cross laying: cross laying carbon fiber unidirectional cloth / carbon fiber mesh at an angle of 0° / 90°; unidirectional laminated needle punching: processing the laid carbon fiber cloth by needle punching technology to form an integrated pre-punctured felt; multi-stage needle punching: adjusting the needle punching density and depth by further multi-stage needle punching treatment; trimming and rolling: performing precise trimming treatment to ensure that the size and shape of the carbon fiber felt meet the design requirements; chemical modification: immersing the carbon fiber felt in an organic strontium modification liquid, washing and drying, obtaining the carbon fiber felt for vanadium redox flow battery VRFB, introducing strontium-containing active groups, and improving its surface activity and electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of long fiber needle punching of carbon fiber felt, in particular to a long fiber needle punching preparation method of carbon fiber felt used for vanadium redox flow battery VRFB. Background Art

[0002] The needle punching process originated from the short-cut fiber manufacturing process in the textile industry. In the field of high-performance fiber fabrics, it mainly refers to a method of using fiber cloth or fiber web as raw materials. Under the high-frequency movement of the needle, the disorderly distributed short fibers in the fiber web are brought into the Z direction by the hook teeth of the needle to prepare the fabric.

[0003] The Chinese patent with the authorization announcement number CN111593478B discloses a method for preparing an asphalt-based general-purpose carbon fiber needle-punched felt, comprising the following steps: 1) preparing asphalt-based general-purpose carbon fiber filaments for standby use; 2) feeding the asphalt-based general-purpose carbon fiber filaments prepared in 1) into an opening machine through a feeding roller to prepare primary asphalt-based general-purpose carbon fiber staples; 3) sending the primary asphalt-based general-purpose carbon fiber staples prepared in 2) to a cotton box by wind, and preparing secondary asphalt-based general-purpose carbon fiber staples through the action of a conveying nail curtain; 4) sending the secondary asphalt-based general-purpose carbon fiber staples prepared in 3) to a cotton drop box, so that the secondary asphalt-based general-purpose carbon fiber staples are evenly laid on the cotton conveying curtain, and then placed in a mesh box, and then evenly laid on the mesh curtain, and under the action of a pre-needling machine, a pre-needled felt is prepared; 5) subjecting the pre-needled felt prepared in 4) to a multi-stage needle-punching treatment, and then trimming and winding.

[0004] A Chinese patent with the authorization announcement number CN110747578B discloses a high-density carbon fiber needle-punched felt, wherein the needle-punched felt is formed by stacking and needle-punching structural units consisting of a carbon fiber web and a carbon fiber widened fabric.

[0005] The Chinese patent with authorization announcement number CN114645462B discloses a high-performance carbon fiber needle-punched preform and a preparation method thereof, comprising: widening ordinary long carbon fiber bundles to form widened continuous long carbon fibers within a preset range of the fiber bundles; using the widened continuous long carbon fibers to prepare short-cut carbon fiber webs; using the widened continuous long carbon fibers and short-cut carbon fibers through needle-punching to prepare various types of unit layers; and composite needle-punching the same type of unit layers to prepare a high-performance carbon fiber needle-punched preform.

[0006] The current needle punching process has the disadvantages of weak interlayer strength of the laminated material, complex process, long cycle and high cost. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a long fiber needle punching preparation method of carbon fiber felt for vanadium redox flow battery VRFB, and the operation steps are as follows:

[0008] S1 Cross-laying: 8 carbon fiber unidirectional fabrics / carbon fiber mesh tires are cross-laid at an angle of 0° / 90° to enhance the structural uniformity and mechanical strength of the finished carbon fiber felt;

[0009] S2 unidirectional laminated needle punching: The above-laid carbon fiber cloth is processed by needle punching technology to form an integrated pre-punched felt. The needle punching promotes the close bonding between fibers and improves the integrity and stability of the material.

[0010] S3 multi-level needling: Through further multi-level needling treatment, the needling density and depth are adjusted to optimize the pore structure and surface properties of the carbon fiber felt to meet the needs of high surface area and low resistance;

[0011] S4 trimming and winding: precise trimming is performed to ensure that the size and shape of the carbon fiber felt meet the design requirements, and winding is performed to prepare for subsequent chemical modification;

[0012] S5 chemical modification: immerse the carbon fiber felt in an organic strontium modification solution to introduce strontium-containing active groups to improve its surface activity and electrochemical properties; then treat it with hydrogen peroxide to oxidize the carbon fiber surface and introduce more oxygen-containing functional groups;

[0013] S6 washing and drying: removing excess chemical reagents by washing and drying to obtain carbon fiber felt for vanadium redox flow battery VRFB.

[0014] The carbon fiber unidirectional cloth described in the above preparation method is made of continuous long fibers and has a surface density of 300-400g / m².

[0015] The carbon fiber mesh described in the above preparation method is prepared by chopping continuous long fibers and carding them into a web, and the surface density is 75-85g / m².

[0016] Wherein, the acupuncture depth of step S2 in the above preparation method is 12-16 mm.

[0017] The acupuncture density in step S3 of the above preparation method is 25-40 pricks·cm -2 .

[0018] The mass concentration of the hydrogen peroxide in the above preparation method is 30-50%, and the added amount is 3-6% of the volume of the organic strontium modified liquid.

[0019] The preparation method of the organic strontium modified liquid described in the above preparation method comprises the following steps:

[0020] H1: Mix 1-3 parts of diethyldithiocarbamic acid, 3-6 parts of strontium nitrate and 100-120 parts of water by weight, react at 30-50°C for 40-100 minutes, and remove water by distillation;

[0021] H2: Add 10-20 parts of dimethyl propylene phosphate-diammonium salt, 0.02-0.54 parts of (ferrocenyl) hexanethiol, and 500-620 parts of ethanol, 10x10 -3 -20x10 -3 0.001-0.02 parts of initiator and lithium diisopropylamide are mixed, and reacted at 70-80° C. for 60-100 minutes to obtain an organic strontium modified liquid.

[0022] The preparation mechanism of the above organic strontium modified liquid:

[0023] Reaction mechanism of H1: Diethyldithiocarbamic acid acts as a ligand to form a complex with strontium ions in strontium nitrate, thereby introducing organic strontium active groups. The formation of this complex helps to improve the chemical properties of the carbon fiber surface, thereby affecting its ultimate electrochemical performance.

[0024] Reaction mechanism of H2: dimethyl propylene phosphate-diammonium salt and (ferrocenyl) hexanethiol undergo a thiol-olefin chemical click addition reaction, and free radicals attack dimethyl propylene phosphate-diammonium salt and (ferrocenyl) hexanethiol, resulting in the growth of the polymer chain.

[0025] Beneficial effects of the present invention:

[0026] 1. Improved tensile strength: The tensile strength of carbon fiber felt reaches 508MPa; this significant strength improvement can be attributed to the better fiber-matrix interface adhesion after carbon fiber surface modification, and the three-dimensional network structure formed by the polymer coating, which helps to disperse and transfer stress more effectively;

[0027] 2. Enhanced interlayer shear strength: The increase in interlayer shear strength to 34MPa indicates that the modified carbon fiber felt has an enhanced ability to resist interlayer sliding; this is mainly due to the cross-linking effect of the organic strontium active groups and polymer chains introduced during the modification process, which enhance the adhesion between the layers and thus improve the overall mechanical properties. DETAILED DESCRIPTION

[0028] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a detailed description in combination with embodiments and comparative examples:

[0029] Tensile performance test: refer to the "Test Method for Tensile Properties of Fiber Reinforced Plastics" (GB / T1447-2006) for testing; interlaminar shear performance test: refer to the "Fiber Reinforced Plastic Short Beam Method for Determination of Interlaminar Shear Strength" (JC / T773-2010) for testing; the testing equipment is Instron1196 electronic universal testing machine, loading is controlled by displacement, and the loading speed is set to 5mm / min.

[0030] Example 1: A method for preparing long fiber acupuncture of carbon fiber felt for vanadium redox flow battery VRFB, wherein the steps are as follows:

[0031] S1 Cross-laying: 8 carbon fiber unidirectional fabrics / carbon fiber mesh tires are cross-laid at an angle of 0° / 90° to enhance the structural uniformity and mechanical strength of the finished carbon fiber felt;

[0032] S2 unidirectional laminated needle punching: The above-laid carbon fiber cloth is processed by needle punching technology to form an integrated pre-punched felt. The needle punching promotes the close bonding between fibers and improves the integrity and stability of the material.

[0033] S3 multi-level needling: Through further multi-level needling treatment, the needling density and depth are adjusted to optimize the pore structure and surface properties of the carbon fiber felt to meet the needs of high surface area and low resistance;

[0034] S4 trimming and winding: precise trimming is performed to ensure that the size and shape of the carbon fiber felt meet the design requirements, and winding is performed to prepare for subsequent chemical modification;

[0035] S5 chemical modification: immerse the carbon fiber felt in an organic strontium modification solution to introduce strontium-containing active groups to improve its surface activity and electrochemical properties; then treat it with hydrogen peroxide to oxidize the carbon fiber surface and introduce more oxygen-containing functional groups;

[0036] S6 washing and drying: removing excess chemical reagents by washing and drying to obtain carbon fiber felt for vanadium redox flow battery VRFB.

[0037] The carbon fiber unidirectional cloth is made of continuous long fibers and has a surface density of 300g / m².

[0038] The carbon fiber web is prepared by chopping continuous long fibers and carding them into a web, and has a surface density of 75g / m².

[0039] The acupuncture depth in step S2 is 12 mm.

[0040] The acupuncture density in step S3 is 25 pricks·cm -2 .

[0041] The mass concentration of the hydrogen peroxide is 30%, and the added amount is 3% of the volume of the organic strontium modified liquid.

[0042] The preparation method of the organic strontium modified liquid comprises the following steps:

[0043] H1: Mix 1 g of diethyldithiocarbamic acid with 3 g of strontium nitrate and 100 g of water, react at 30°C for 40 minutes, and remove water by distillation;

[0044] H2: Add 10g dimethyl propylene phosphate diammonium salt, 0.02g (ferrocenyl) hexanethiol, and 500g ethanol, 10x10 -3 0.001 g of lithium diisopropylamide were mixed and reacted at 70° C. for 60 minutes to obtain an organic strontium modified liquid.

[0045] Example 2: A method for preparing long fiber acupuncture of carbon fiber felt for vanadium redox flow battery VRFB, wherein the steps are as follows:

[0046] S1 Cross-laying: 8 carbon fiber unidirectional fabrics / carbon fiber mesh tires are cross-laid at an angle of 0° / 90° to enhance the structural uniformity and mechanical strength of the finished carbon fiber felt;

[0047] S2 unidirectional laminated needle punching: The above-laid carbon fiber cloth is processed by needle punching technology to form an integrated pre-punched felt. The needle punching promotes the close bonding between fibers and improves the integrity and stability of the material.

[0048] S3 multi-level needling: Through further multi-level needling treatment, the needling density and depth are adjusted to optimize the pore structure and surface properties of the carbon fiber felt to meet the needs of high surface area and low resistance;

[0049] S4 trimming and winding: precise trimming is performed to ensure that the size and shape of the carbon fiber felt meet the design requirements, and winding is performed to prepare for subsequent chemical modification;

[0050] S5 chemical modification: immerse the carbon fiber felt in an organic strontium modification solution to introduce strontium-containing active groups to improve its surface activity and electrochemical properties; then treat it with hydrogen peroxide to oxidize the carbon fiber surface and introduce more oxygen-containing functional groups;

[0051] S6 washing and drying: removing excess chemical reagents by washing and drying to obtain carbon fiber felt for vanadium redox flow battery VRFB.

[0052] The carbon fiber unidirectional cloth is made of continuous long fibers and has a surface density of 350g / m².

[0053] The carbon fiber web is prepared by chopping continuous long fibers and carding them into a web, and has a surface density of 80 g / m².

[0054] The acupuncture depth in step S2 is 13 mm.

[0055] The acupuncture density in step S3 is 30 pricks·cm -2 .

[0056] The mass concentration of the hydrogen peroxide is 35%, and the added amount is 4% of the volume of the organic strontium modified liquid.

[0057] The preparation method of the organic strontium modified liquid comprises the following steps:

[0058] H1: Mix 2 g of diethyldithiocarbamic acid with 4 g of strontium nitrate and 105 g of water, react at 35°C for 60 minutes, and remove water by distillation;

[0059] H2: Add 13g dimethyl propylene phosphate diammonium salt, 0.2g (ferrocenyl) hexanethiol, and 540g ethanol, mix, 13x10 -3 0.01 g of initiator and 0.01 g of lithium diisopropylamide were mixed and reacted at 75° C. for 70 minutes to obtain an organic strontium modified liquid.

[0060] Example 3: A method for preparing long fiber acupuncture of carbon fiber felt for vanadium redox flow battery VRFB, wherein the steps are as follows:

[0061] S1 Cross-laying: 8 carbon fiber unidirectional fabrics / carbon fiber mesh tires are cross-laid at an angle of 0° / 90° to enhance the structural uniformity and mechanical strength of the finished carbon fiber felt;

[0062] S2 unidirectional laminated needle punching: The above-laid carbon fiber cloth is processed by needle punching technology to form an integrated pre-punched felt. The needle punching promotes the close bonding between fibers and improves the integrity and stability of the material.

[0063] S3 multi-level needling: Through further multi-level needling treatment, the needling density and depth are adjusted to optimize the pore structure and surface properties of the carbon fiber felt to meet the needs of high surface area and low resistance;

[0064] S4 trimming and winding: precise trimming is performed to ensure that the size and shape of the carbon fiber felt meet the design requirements, and winding is performed to prepare for subsequent chemical modification;

[0065] S5 chemical modification: immerse the carbon fiber felt in an organic strontium modification solution to introduce strontium-containing active groups to improve its surface activity and electrochemical properties; then treat it with hydrogen peroxide to oxidize the carbon fiber surface and introduce more oxygen-containing functional groups;

[0066] S6 washing and drying: removing excess chemical reagents by washing and drying to obtain carbon fiber felt for vanadium redox flow battery VRFB.

[0067] The carbon fiber unidirectional cloth is made of continuous long fibers and has a surface density of 350g / m².

[0068] The carbon fiber web is prepared by chopping continuous long fibers and carding them into a web, and has a surface density of 80 g / m².

[0069] The acupuncture depth in step S2 is 15 mm.

[0070] The acupuncture density in step S3 is 35 punctures·cm -2 .

[0071] The mass concentration of the hydrogen peroxide is 45%, and the added amount is 5% of the volume of the organic strontium modified liquid.

[0072] The preparation method of the organic strontium modified liquid comprises the following steps:

[0073] H1: Mix 2 g of diethyldithiocarbamic acid with 5 g of strontium nitrate and 115 g of water, react at 45°C for 80 minutes, and remove water by distillation;

[0074] H2: Add 18g dimethyl propylene phosphate diammonium salt, 0.4g (ferrocenyl) hexanethiol, and 600g ethanol, 18x10 -3 0.015 g of initiator and 0.015 g of lithium diisopropylamide were mixed and reacted at 75° C. for 90 minutes to obtain an organic strontium modified liquid.

[0075] Example 4: A method for preparing long fiber acupuncture of carbon fiber felt for vanadium redox flow battery VRFB, wherein the steps are as follows:

[0076] S1 Cross-laying: 8 carbon fiber unidirectional fabrics / carbon fiber mesh tires are cross-laid at an angle of 0° / 90° to enhance the structural uniformity and mechanical strength of the finished carbon fiber felt;

[0077] S2 unidirectional laminated needle punching: The above-laid carbon fiber cloth is processed by needle punching technology to form an integrated pre-punched felt. The needle punching promotes the close bonding between fibers and improves the integrity and stability of the material.

[0078] S3 multi-level needling: Through further multi-level needling treatment, the needling density and depth are adjusted to optimize the pore structure and surface properties of the carbon fiber felt to meet the needs of high surface area and low resistance;

[0079] S4 trimming and winding: precise trimming is performed to ensure that the size and shape of the carbon fiber felt meet the design requirements, and winding is performed to prepare for subsequent chemical modification;

[0080] S5 chemical modification: immerse the carbon fiber felt in an organic strontium modification solution to introduce strontium-containing active groups to improve its surface activity and electrochemical properties; then treat it with hydrogen peroxide to oxidize the carbon fiber surface and introduce more oxygen-containing functional groups;

[0081] S6 washing and drying: removing excess chemical reagents by washing and drying to obtain carbon fiber felt for vanadium redox flow battery VRFB.

[0082] The carbon fiber unidirectional cloth is made of continuous long fibers and has a surface density of 400g / m².

[0083] The carbon fiber web is prepared by chopping continuous long fibers and carding them into a web, and has a surface density of 85g / m².

[0084] The acupuncture depth in step S2 is 16 mm.

[0085] The acupuncture density in step S3 is 40 punctures·cm -2 .

[0086] The mass concentration of the hydrogen peroxide is 50%, and the added amount is 6% of the volume of the organic strontium modified liquid.

[0087] The preparation method of the organic strontium modified liquid comprises the following steps:

[0088] H1: 3 g of diethyldithiocarbamic acid, 6 g of strontium nitrate and 120 g of water were mixed, reacted at 50°C for 100 minutes, and the water was distilled off;

[0089] H2: Add 20g dimethyl propylene phosphate diammonium salt, 0.54g (ferrocenyl) hexanethiol, and 620g ethanol, mix, 20x10 -3 0.02 g of lithium diisopropylamide were mixed and reacted at 80° C. for 100 minutes to obtain an organic strontium modified liquid.

[0090] Comparative Example 1: This example is a comparative example of Example 1, which is basically the same as Example 1, except that no organic strontium modification liquid is added.

[0091] Comparative Example 2: This example is a comparative example of Example 1, which is basically the same as Example 1, except that diethyldithiocarbamic acid is not added.

[0092] Comparative Example 3: This example is a comparative example of Example 1, which is basically the same as Example 1, except that (ferrocenyl) hexanethiol is not added.

[0093] Table 1: Test results of various embodiments and comparative examples

[0094]

[0095] Through the data analysis of the above embodiments and comparative examples, the organic strontium modified liquid prepared by the present invention can effectively improve the tensile strength of the carbon fiber felt, and at the same time enhance the interlaminar shear strength, thereby improving the overall mechanical properties.

[0096] The above are only embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing long fiber needle punching of carbon fiber felt for vanadium redox flow battery VRFB, Features: The operation steps are: S1 cross-laying: 8 carbon fiber unidirectional fabrics / carbon fiber mesh tires are cross-laid at an angle of 0° / 90°; S2 unidirectional laminated needle punching: the above-laid carbon fiber cloth is processed by needle punching technology to form an integrated pre-punched felt; S3 multi-level needling: Through further multi-level needling treatment, the needling density and depth are adjusted to optimize the pore structure and surface properties of the carbon fiber felt to meet the needs of high surface area and low resistance; S4 trimming and winding: precise trimming is performed to ensure that the size and shape of the carbon fiber felt meet the design requirements, and winding is performed to prepare for subsequent chemical modification; S5 chemical modification: immerse the carbon fiber felt in an organic strontium modification solution to introduce strontium-containing active groups to improve its surface activity and electrochemical properties; then treat it with hydrogen peroxide to oxidize the carbon fiber surface and introduce more oxygen-containing functional groups; S6 washing and drying: removing excess chemical reagents by washing and drying to obtain carbon fiber felt for vanadium redox flow battery VRFB; Preparation method of the organic strontium modified liquid The following steps are involved: H1: Mix 1-3 parts of diethyldithiocarbamic acid, 3-6 parts of strontium nitrate and 100-120 parts of water by weight, react at 30-50°C for 40-100 minutes, and remove water by distillation; H2: Add 10-20 parts of dimethyl propylene phosphate-diammonium salt, 0.02-0.54 parts of (ferrocenyl) hexanethiol, 500-620 parts of ethanol, 10x10-3-20x10-3 parts of initiator, 0.001-0.02 parts of lithium diisopropylamide, react at 70-80°C for 60-100 minutes to obtain an organic strontium modified liquid.

2. The long fiber needle punching preparation method of carbon fiber felt for vanadium redox flow battery VRFB according to claim 1, Features: The carbon fiber unidirectional cloth is made of continuous long fibers and has a surface density of 300-400g / m².

3. The long fiber needle punching preparation method of carbon fiber felt for vanadium redox flow battery VRFB according to claim 1, Features: The carbon fiber mesh is prepared by chopping continuous long fibers and carding them into a mesh, and has a surface density of 75-85g / m².

4. The long fiber needle punching preparation method of carbon fiber felt for vanadium redox flow battery VRFB according to claim 1, Features: The acupuncture depth in step S2 is 12-16 mm.

5. The long fiber needle punching preparation method of carbon fiber felt for vanadium redox flow battery VRFB according to claim 1, Features: The acupuncture density in step S3 is 25-40 punctures·cm -2 .