Sublimation preparation process of double-sided roughened solid oxide fuel cell electrolyte membrane

Through dry pressure, low temperature sublimation and calcining processes, a dense and uniform electrolyte film with both sides was prepared, which solved the life and cost of SOFC cells and significantly improved the battery performance and production efficiency.

CN118522929BInactive Publication Date: 2024-12-03TAIYUAN INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410654636.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The high operating temperature of existing solid oxide fuel cells (SOFCs) leads to a reduced battery life, the performance requirements of electrode materials and connector materials increase production costs, and it is difficult to prepare double-sided rough electrolyte films, affecting battery performance.

Method used

Using the process steps of dry pressure, low temperature sublimation and calcination, a dense and uniform electrolyte film with both sides is prepared by multi-layer co-pressure molding of the base material, buffer layer and electrolyte material, combined with medium and low temperature sublimation and high temperature calcination.

Benefits of technology

It significantly improves the close contact between the electrode and the electrolyte material, improves battery performance, simplifies process operations, is suitable for the preparation of electrolyte films of various thicknesses, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118522929B_ABST
    Figure CN118522929B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of fuel cell technology, and in particular to a sublimation method preparation process for a double-sided rough solid oxide fuel cell electrolyte film. The sublimation method preparation process adopts the steps of dry pressing-low temperature sublimation-calcination to prepare a double-sided rough solid oxide fuel cell electrolyte film. The overall operation is simple, and it is suitable for preparing double-sided rough, dense, and uniform electrolyte films of various thicknesses, which significantly improves the close contact between electrodes and electrolyte materials and can improve battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fuel cells, and in particular to a sublimation process for preparing a double-sided rough solid oxide fuel cell electrolyte film. Background Art

[0002] Solid oxide fuel cell (SOFC) is a device that directly converts the chemical energy of fuel into electrical energy at high temperature (600-1000℃). SOFC has the following outstanding advantages: high energy conversion efficiency; wide range of fuel adaptability; no need to use precious metals as catalysts, low cost; all-solid-state structure, improved system safety factor, enhanced operational stability; low greenhouse gas emissions; wide range of applications. Therefore, it has received more and more attention. The existing SOFC has a high operating temperature, which will accelerate the mutual reaction and diffusion of the battery components during battery operation, reduce the service life of the battery, and at the same time put forward higher requirements on the performance of materials such as electrode materials and connectors, resulting in increased production costs and affecting the commercial competitiveness of SOFC.

[0003] The power density and output performance of the battery are closely related to the internal resistance of the battery. The internal resistance of the battery is mainly determined by the bulk resistance of the electrolyte and the three-phase interface resistance between the electrolyte and the anode. A large internal resistance has a negative impact on the power density and output performance of the battery, and the thickness of the electrolyte film is one of the factors affecting the internal resistance of the battery. In the prior art, the powder dry pressing method is often used to prepare the electrolyte film of the electrolyte-supported fuel cell. The powder sample that has been dried or roasted, ground and mixed evenly is placed in a special mold and pressed into a sample sheet by a press under a certain pressure, which is called powder tableting. The powder is compacted into a thin sheet. During the powder tableting process, the powder needs to be spread in the mold first. The prepared electrolyte sheet is thicker. In order to reduce the resistance, the surface needs to be polished before use, which can easily cause damage to the electrolyte sheet.

[0004] The applicant's prior patent "A method for preparing a zirconium-based electrolyte film for an electrolyte-supported solid oxide fuel cell" patent number 2018110564070, prepared an electrolyte-supported solid oxide fuel cell zirconium-based electrolyte film by dry pressing / heating / quenching / calcination method. It is a single-sided rough YSZ film. The rough electrolysis is conducive to the close contact between the electrode and the electrolyte, and accelerates the mass transfer during the electrolysis process, thereby improving the battery performance of the YSZ-supported SOFC. The patent has made progress in the ultra-thin and uniform preparation of zirconium-based electrolytes, but it is difficult to obtain a double-sided rough electrolyte film. Summary of the invention

[0005] In order to make up for the shortcomings of the prior art, the present invention provides a sublimation method preparation process for a double-sided rough solid oxide fuel cell electrolyte film. The process is simple to operate and is suitable for preparing double-sided rough, dense and uniform electrolyte films of various thicknesses. It significantly improves the close contact between electrodes and electrolyte materials, improves battery performance, and solves the problems existing in the prior art.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:

[0007] A sublimation preparation process for a double-sided rough solid oxide fuel cell electrolyte film comprises the steps of dry pressing, low-temperature sublimation and calcination.

[0008] Furthermore, the specific steps of the sublimation process for preparing the double-sided roughened solid oxide fuel cell electrolyte membrane are as follows:

[0009] (1) grinding a base material that is easily sublimated at low and medium temperatures uniformly, and molding it into sheets to obtain a thin sheet;

[0010] (2) evenly spreading a buffer layer granular material that is stable at medium and low temperatures and has high hardness on the surface of the thin slice obtained in step (1), and co-pressing the material to form a base / buffer layer double-layer green body consisting of a base layer and a buffer layer;

[0011] (3) evenly spreading the powder material for preparing the electrolyte film on the surface of the buffer layer of the substrate / buffer layer double-layer green body obtained in step (2), and co-pressing to form a substrate / buffer layer / electrolyte three-layer green body having a substrate layer, a buffer layer, and an electrolyte layer;

[0012] (4) spreading the buffer layer granular material which is stable at medium and low temperatures and has high hardness on the electrolyte surface of the substrate / buffer layer / electrolyte three-layer green body obtained in step (3), and co-pressing to form a substrate / buffer layer / electrolyte layer / buffer layer four-layer green body;

[0013] (5) evenly spreading a substrate material that is easily sublimated at medium and low temperatures on the surface of the buffer layer of the four-layer green body of substrate / buffer layer / electrolyte layer / buffer layer obtained in step (4), and co-pressing to form a five-layer green body of substrate / buffer layer / electrolyte layer / buffer layer / substrate;

[0014] (6) placing the substrate / buffer layer / electrolyte layer / buffer layer / substrate five-layer green body obtained in step (5) on a zirconia plate, placing it on a hot plate at a suitable temperature for several hours to sublime the substrate material, and obtaining an electrolyte layer green body;

[0015] (7) After being placed in a high-temperature muffle furnace for high-temperature calcination, a dense and uniform double-sided rough electrolyte-supported solid oxide fuel cell electrolyte membrane is obtained.

[0016] Furthermore, the base material of step (1) and step (5) is camphor balls, naphthalene or iodine; the particle size is ≥100 mesh; the molding pressure of step (1) is 80-90 MPa, and the holding time is 20 s.

[0017] Furthermore, the medium-low temperature in step (2) refers to 50° C.-200° C.; the high hardness refers to the Mohs hardness range of 3-8.

[0018] Furthermore, the buffer layer particle material of step (2) and step (4) is quartz sand, calcium carbonate particles, sodium silicate particles or calcium silicate particles, with a particle size of ≥80 mesh; the co-pressing molding molding pressure is 3-10MPa, and the holding time is 10s.

[0019] Furthermore, the powder material in step (3) is yttria-stabilized zirconia (YSZ), doped CeO2 or doped LaGaO3; and the particle size is ≥100 mesh.

[0020] Furthermore, the molding pressure of the co-pressing molding in step (3) is 90-100 MPa, and the holding time is 30 s.

[0021] Furthermore, the co-pressing molding pressure in step (5) is 90-110 MPa, and the holding time is 40 s.

[0022] Furthermore, in step (6), the heating temperature of the electric heating plate is 70-120° C., and the heating time is 1-2 h.

[0023] Furthermore, in step (6), the heating temperature of the electric heating plate is 70-86° C., the heating time is 1-2 h, and preferably the heating time is 1 h.

[0024] Furthermore, in step (7), the high temperature calcination temperature is 1400° C., the calcination time is 5 h, and the heating rate is 5° C. / min.

[0025] Beneficial effects of the present invention:

[0026] 1. The process of the present invention is simple to operate and can be used to batch prepare rough, dense and uniform electrolyte films with various thicknesses on both sides.

[0027] 2. Compared with the traditional dry pressing method, the thicker film is calcined at high temperature to make it have a certain hardness, and then the whole process of calcining it with sandpaper after film treatment is to be calcined twice at high temperature. The present invention adopts sublimation method to prepare, and the base material-camphor that is easy to sublimate under medium and low temperature can complete sublimation at 80 degrees, and the addition of the buffer layer granular material between the camphor layer and YSZ is conducive to the removal of the camphor layer on the one hand, and the buffer layer granular material with uniform thickness can improve the surface roughness of the YSZ layer on the other hand. If the electrolyte film of the three-layer structure of camphor layer / YSZ / camphor layer is prepared by the traditional dry pressing method, after heating, the camphor layer is dense after dry pressing, even if the camphor layer cannot be completely sublimated under high temperature (1200 degrees), it shows a vitrification trend, and the corresponding product cannot be obtained. Compared with the single-sided rough YSZ film prepared by the dry pressing / heating / quenching / calcination method disclosed in the applicant's previous patent, the double-sided rough solid oxide fuel cell electrolyte film of the present invention, on the one hand, belongs to a double-sided rough electrolyte film with obvious differences, and the preparation operation process only requires three steps of dry pressing-low temperature sublimation-calcination, and the specific preparation process is obviously different. On the other hand, the solid oxide fuel cell electrolyte film prepared by the present invention is more conducive to the close contact between the electrode and the electrolyte, accelerates the mass transfer in the electrolysis process, and significantly improves the battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The surface roughness of both sides of the electrolyte film measured by a 3D optical profiler in Example 1 of the present invention;

[0029] Figure 2 The surface roughness of both sides of the electrolyte film prepared by the traditional dry pressing method was measured by a 3D optical profilometer;

[0030] Figure 3 The electrochemical performance of the battery prepared by the electrolyte film of Example 1 of the present invention and the electrolyte film-based battery prepared by the conventional dry pressing method under SOFC mode;

[0031] Figure 4 The electrochemical performance of the battery prepared using the electrolyte film of Example 1 of the present invention under the SOEC mode at different temperatures;

[0032] Figure 5 Electrochemical performance of electrolyte thin film-based batteries prepared by traditional dry pressing method at different temperatures in SOEC mode;

[0033] Figure 6 The electrochemical performance of a battery prepared by using the electrolyte film of Example 1 of the present invention and an electrolyte film-based battery prepared by a conventional dry pressing method at 850° C. in SOEC mode;

[0034] in, Figure 3-Figure 6The "sublimation, traditional" marked in the figure correspond to the solid oxide fuel cell electrolyte membrane (or a battery made therefrom) of Example 1 of the present invention and the electrolyte membrane (or electrolyte membrane-based battery) prepared by the traditional dry pressing method, respectively. DETAILED DESCRIPTION

[0035] In order to clearly illustrate the technical features of this solution, the present invention is described in detail below through specific implementation methods and in conjunction with the accompanying drawings. The scope of the present invention is not limited to the following embodiments. Professionals in the field can understand that various changes and modifications can be made to the present invention without departing from the spirit and scope of the present invention.

[0036] The instruments, reagents, materials, etc. involved in the following embodiments, unless otherwise specified, are all conventional instruments, reagents, materials, etc. in the prior art and can be obtained through regular commercial channels. The experimental methods, detection methods, etc. involved in the following embodiments, unless otherwise specified, are all conventional experimental methods, detection methods, etc. in the prior art.

[0037] Example 1

[0038] A sublimation process for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane includes the steps of dry pressing, low-temperature sublimation and calcination. Camphor is used as the base material and YSZ (8% yttrium-stabilized zirconium dioxide) is used as the electrolyte to prepare the YSZ electrolyte membrane. The specific operation steps are as follows:

[0039] (1) Grind camphor evenly, weigh 0.08 g of the powder and press it into a sheet with a thickness of about 100 μm using a tablet press with a diameter of 15 mm and a pressure of 80 MPa for 20 s;

[0040] (2) using an 80-mesh sieve to evenly spread a small amount of silicon dioxide on the surface of the pressed camphor flakes, and gently rotating the mold column to make the silicon dioxide more evenly distributed; using a press to co-press and mold, the molding pressure is 3-10 MPa, and the holding time is 10 s;

[0041] (3) 0.2 g of electrolyte YSZ powder was evenly spread on the surface of the sheet, and co-pressed at 90 MPa for 30 s to form a substrate / buffer layer / electrolyte three-layer green body;

[0042] (4) using an 80-mesh sieve to evenly spread a small amount of silicon dioxide on the surface of the pressed electrolyte sheet, and gently rotating the mold column to make the silicon dioxide distribution more uniform; using a press to co-press and mold, the molding pressure is 10 MPa, and the holding time is 10 s;

[0043] (5) evenly spreading 0.08 g of camphor powder on the surface of the silicon dioxide obtained in step (4), and co-pressing the silicon dioxide on a tablet press at a pressure of 100 MPa for 40 seconds to form a five-layer green body of substrate / buffer layer / electrolyte layer / buffer layer / substrate;

[0044] (6) placing a five-layer green body of substrate / buffer layer / electrolyte layer / buffer layer / substrate on a zirconia plate and heating it on a hot plate at 85° C. for 1 h to sublimate the camphor, thereby forming a single electrolyte YSZ layer in the five-layer green body;

[0045] (7) The single electrolyte YSZ layer was calcined in a muffle furnace at 1400°C for 5 h with a heating rate of 5°C / min to obtain a double-sided rough and dense and uniform electrolyte-supported solid oxide fuel cell electrolyte membrane.

[0046] Gold spraying was performed on both sides of the electrolyte film prepared above, and the surface roughness was tested using a 3D optical profiler. Figure 1 As shown in FIG. 1 , the root mean square roughness of the two sides of the electrolyte film prepared above was measured to be 12.364 and 14.295 μm, respectively. In comparison, the root mean square roughness of the two sides of the electrolyte film prepared by the conventional direct dry pressing method (0.2 g YSZ powder) was 0.325 and 0.548 μm, respectively. Figure 2 shown.

[0047] Example 2

[0048] A sublimation process for preparing a double-sided rough solid oxide fuel cell electrolyte membrane, using iodine as the base material and YSZ (8% yttrium-stabilized zirconium dioxide) as the electrolyte, to prepare a YSZ electrolyte membrane. The specific steps are as follows:

[0049] (1) Grind iodine evenly, weigh 0.08 g of powder and press it into a sheet with a thickness of about 100 μm using a tablet press with a diameter of 15 mm and a pressure of 80 MPa for 20 s;

[0050] (2) using an 80-mesh sieve to evenly spread a small amount of calcium carbonate particles on the surface of the pressed iodine flakes, and gently rotating the mold column to make the calcium carbonate particles more evenly distributed; using a press to co-press and mold, the molding pressure is 3-10 MPa, and the holding time is 10 s;

[0051] (3) 0.2 g of electrolyte YSZ powder was evenly spread on the surface of the thin slice, and the pressure was maintained at 100 MPa for 30 s, and co-pressed to form a substrate / buffer layer / electrolyte three-layer green body;

[0052] (4) using an 80-mesh sieve to evenly spread a small amount of calcium carbonate particles on the surface of the pressed electrolyte sheet, and gently rotating the mold column to make the calcium carbonate particles more evenly distributed; using a press to co-press and mold, the molding pressure is 3-10 MPa, and the holding time is 10 s;

[0053] (5) evenly spreading 0.08 g of iodine powder on the surface of the calcium carbonate particles obtained in step (4), and co-pressing on a tablet press at a pressure of 110 MPa for 40 seconds to form a five-layer green body of substrate / buffer layer / electrolyte layer / buffer layer / substrate;

[0054] (6) placing a five-layer green body of substrate / buffer layer / electrolyte layer / buffer layer / substrate on a zirconia plate and heating it on a hot plate at 75° C. for 1 h to sublimate iodine, thereby forming a single electrolyte YSZ layer in the five-layer green body;

[0055] (7) The electrolyte YSZ alone was calcined in a muffle furnace at 1400°C for 5 h with a heating rate of 5°C / min to obtain a double-sided rough and dense and uniform electrolyte-supported solid oxide fuel cell electrolyte membrane.

[0056] Example 3

[0057] A cathode and an anode electrode layer were sprayed on both sides of a YSZ electrolyte film prepared by a conventional dry pressing method to prepare a battery for comparison with a battery made of the solid oxide fuel cell electrolyte film prepared in Example 1.

[0058] The electrochemical performance of the battery was tested under H2 atmosphere at 850°C using an electrochemical workstation. Figure 3 , 4 As shown, the current-voltage (power) curve is obtained. Figure 3 It can be seen that the highest power density of the electrolyte-based battery prepared by the traditional dry pressing method is 0.35 W cm -2 , the maximum current density is higher than 1.37A cm -2 Under the same conditions, the improved battery made by the sublimation solid oxide fuel cell electrolyte membrane of the present invention has greatly improved performance, and its maximum power density and maximum current density are increased to 0.46W cm -2 and 2.31A cm -2 , see Figure 4 .

[0059] The IV curves of the battery for electrolysis of CO2 at different temperatures of 750°C, 800°C, and 850°C were tested using an electrochemical workstation. It can be found that at the same temperature, the current density increases with the increase of the applied voltage. At 800°C and 1.2V, the current density is 0.34A cm -2 , while the current density increased to 0.78 A cm at 1.6 V.-2 In addition, it can be found that compared with the electrolyte-based battery prepared by the traditional method, under the same conditions, the improved battery prepared by the sublimation method solid oxide fuel cell electrolyte membrane of the present invention has significantly improved CO2 electrolysis performance, such as Figure 5 As shown in FIG. 1 , the current density of the improved battery made of the sublimation solid oxide fuel cell electrolyte membrane of the present invention at 1.2V and 1.6V is increased to 0.48 and 1.17A cm respectively. -2 .like Figure 6 As shown in FIG. 1 , the IV curves of the conventional battery and the improved battery made of the sublimation solid oxide fuel cell electrolyte membrane of the present invention at 850°C for electrolysis of CO2 are shown. It can be seen that compared with the conventional battery, the improved battery made of the sublimation solid oxide fuel cell electrolyte membrane of the present invention has a significant improvement in electrolysis of CO2. For example, at 1.6V, the current densities of the conventional battery and the improved battery made of the sublimation solid oxide fuel cell electrolyte membrane of the present invention are 1.32 and 1.81 Acm, respectively. -2 , performance improved by 37%.

[0060] The above specific implementation manner cannot be used as a limitation on the protection scope of the present invention. For those skilled in the art, any substitution, improvement or change made to the implementation manner of the present invention falls within the protection scope of the present invention.

[0061] The matters not described in detail in the present invention are all known technologies to those skilled in the art.

Claims

1. A sublimation process for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane, characterized in that: The process includes the steps of dry pressing, low temperature sublimation and calcination, and the specific steps are as follows: (1) grinding a base material that is easily sublimated at low and medium temperatures uniformly, and molding it into sheets to obtain a thin sheet; (2) evenly spreading a buffer layer granular material that is stable at medium and low temperatures and has high hardness on the surface of the thin slice obtained in step (1), and co-pressing the material to form a base / buffer layer double-layer green body consisting of a base layer and a buffer layer; (3) evenly spreading the powder material for preparing the electrolyte film on the surface of the buffer layer of the substrate / buffer layer double-layer green body obtained in step (2), and co-pressing to form a substrate / buffer layer / electrolyte three-layer green body having a substrate layer, a buffer layer, and an electrolyte layer; (4) spreading the buffer layer granular material which is stable at medium and low temperatures and has high hardness on the electrolyte surface of the substrate / buffer layer / electrolyte three-layer green body obtained in step (3), and co-pressing to form a substrate / buffer layer / electrolyte layer / buffer layer four-layer green body; (5) evenly spreading a substrate material that is easily sublimated at medium and low temperatures on the surface of the buffer layer of the four-layer green body of substrate / buffer layer / electrolyte layer / buffer layer obtained in step (4), and co-pressing to form a five-layer green body of substrate / buffer layer / electrolyte layer / buffer layer / substrate; (6) placing the substrate / buffer layer / electrolyte layer / buffer layer / substrate five-layer green body obtained in step (5) on a zirconia plate, placing it on a hot plate and heating it at a heating temperature of 70-120° C. for 1-2 h to sublime the substrate material, thereby obtaining an electrolyte layer green body; (7) After being placed in a high-temperature muffle furnace for high-temperature calcination, a dense and uniform solid oxide fuel cell electrolyte membrane with rough electrolyte support on both sides is obtained; The base material of step (1) and step (5) is camphor balls, naphthalene or iodine; the buffer layer particle material of step (2) and step (4) is quartz sand, calcium carbonate particles, sodium silicate particles or calcium silicate particles.

2. The sublimation method for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane according to claim 1, characterized in that: The particle size of the base material in step (1) and step (5) is ≥100 mesh; the molding pressure in step (1) is 80-90 MPa, and the holding time is 20 s.

3. The sublimation method for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane according to claim 1, characterized in that: The particle size of the buffer layer granular material in step (2) and step (4) is ≥80 mesh; the molding pressure of co-pressing is 3-10MPa, and the holding time is 10s.

4. The sublimation method for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane according to claim 1, characterized in that: The powder material of step (3) is yttria-stabilized zirconia, doped CeO2 or doped LaGaO3; the particle size is ≥100 mesh.

5. The sublimation method for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane according to claim 1, characterized in that: The molding pressure of the co-pressing molding in step (3) is 90-100 MPa, and the holding time is 30 s.

6. The sublimation method for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane according to claim 1, characterized in that: The molding pressure of the co-pressing molding in step (4) is 3-10 MPa, and the holding time is 10 s.

7. The sublimation method for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane according to claim 1, characterized in that: The molding pressure of the co-pressing molding in step (5) is 90-110 MPa, and the holding time is 40 s.

8. The sublimation method for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane according to claim 1, characterized in that: The heating temperature of the electric heating plate in step (6) is 70-86°C.

9. The sublimation method for preparing a double-sided roughened solid oxide fuel cell electrolyte membrane according to claim 1, characterized in that: The high-temperature calcination temperature of step (7) is 1400°C, the calcination time is 5h, and the heating rate is 5°C / min.

Citation Information

Patent Citations

  • Compound film electrode of catalytic layer supported proton exchange film fuel cells and method for making same

    CN101038968A

  • Preparation method of electrolyte-supported solid oxide fuel cell zirconium-based electrolyte thin film

    CN109346752A

  • Preparation method of barium zirconate-based electrolyte film

    CN111099894A

  • Electrochemical cell and method of manufacturing the same

    GB202219366D0

  • Manufacturing method of polymer electrolyte membrane

    JP2012079467A