A piezoelectric antibacterial material, its preparation method and application

By preparing Ba1-xCaxTiySnzZrnO3 piezoelectric antibacterial material and combining it with tannic acid-modified bentonite, the problem of insufficient mechanical properties of piezoelectric antibacterial materials was solved, achieving a highly efficient and long-lasting antibacterial effect, especially in the application of bentonite-based antibacterial cat litter.

CN118527136BActive Publication Date: 2026-11-10宁城县工业和数字经济产业促进中心 +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410586846.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-13
Publication Date
2026-11-10
Estimated Expiration
2044-05-13

AI Technical Summary

Technical Problem

Existing piezoelectric antibacterial materials have limited mechanical properties. Powdered piezoelectric materials are difficult to guarantee effectiveness in practical use, and their low piezoelectric performance results in low efficiency in utilizing mechanical energy in the environment.

Method used

Using Ba1-xCaxTiySnzZrnO3 material, a piezoelectric antibacterial material with high voltage effect was prepared by controlling the ratio of x, y, and z and combining it with ball milling. Furthermore, bentonite was modified with tannic acid to improve its bonding strength with bentonite and directional adsorption, ensuring effective polarization in bentonite-based antibacterial cat litter.

Benefits of technology

The mechanical properties and antibacterial effect of piezoelectric antibacterial materials have been improved, achieving long-lasting and stable antibacterial performance in bentonite-based antibacterial cat litter, with a sterilization rate of over 99%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118527136B_ABST
    Figure CN118527136B_ABST
Patent Text Reader

Abstract

This invention relates to antibacterial materials, and more particularly to a piezoelectric antibacterial material, its preparation method, and its application. The preparation method includes: according to the stoichiometric formula Ba... 1‑x Ca x Ti y Sn z Zr n O3 is prepared by mixing barium, calcium, titanium, tin, and / or zirconium sources, and then adding ball milling media for initial ball milling to obtain a pre-powder. The pre-powder is dried and calcined at 1200–1280°C for 3.5–4.5 hours, followed by a second ball milling to obtain the antibacterial piezoelectric material. Wherein: y + z + n = 1, where 0 < x < 1, 0 < y < 1, 0 ≤ z < 1, and 0 ≤ n < 1. This invention features a simple preparation process and low cost. The prepared material exhibits good mechanical properties and biocompatibility, and displays excellent long-lasting antibacterial performance under environmental mechanical stimulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to antibacterial materials, and more particularly to a piezoelectric antibacterial material, its preparation method, and its application. Background Technology

[0002] Piezoelectric catalysis technology has attracted widespread attention as a novel advanced oxidation method. This sterilization method can completely kill bacteria and catalytically degrade toxic substances within bacterial cells, mineralizing them into carbon dioxide and water without causing secondary pollution, making it an ideal sterilization technology. Piezoelectric catalytic sterilization utilizes the superoxide radicals (·O₂) generated on the catalyst surface under external mechanical stimulation by piezoelectric materials with non-centrosymmetry. 2- Piezoelectric catalytic sterilization technology utilizes reactive groups such as hydroxyl radicals (·OH), singlet oxygen (1O2), and hydrogen peroxide (H2O2). These highly oxidizing active ingredients initially attack phospholipids, proteins, and peptidoglycans on the cell wall, oxidizing the cell wall and disrupting its selective permeability. This allows them to penetrate the cell wall, destroy the cell membrane, and cause intracellular substances to leak out, leading to bacterial death. Additionally, these active ingredients oxidize coenzyme A, which is closely related to cellular metabolism; the disruption of this metabolism causes bacterial death. However, piezoelectric catalytic sterilization technology is still in its early stages, and its specific mechanism of action remains unclear. Furthermore, the piezoelectric properties of materials used for piezoelectric sterilization are relatively low, which significantly limits their effective utilization of mechanical energy in the environment. Moreover, existing piezoelectric materials generally exhibit the characteristic of generating different charges on different surfaces under stress. For example, some piezoelectric ceramic materials will generate two opposite charges on their surface when subjected to pressure, and the polarity will reverse when subjected to tension. At the microscopic level, powdered piezoelectric materials are correlated with their stressed crystal planes. However, in actual use, it is impossible to guarantee that the stressed crystal planes of powdered piezoelectric materials will meet expectations, resulting in very limited actual use effects. Summary of the Invention

[0003] To address the limitations of existing piezoelectric antibacterial materials in terms of mechanical properties and the difficulty in ensuring the effectiveness of powdered piezoelectric materials in practical applications, this invention provides a piezoelectric antibacterial material, a method for preparing the piezoelectric antibacterial material, and a practical and effective application method for the prepared powdered piezoelectric antibacterial material.

[0004] The purpose of this invention is:

[0005] I. Improve the mechanical properties of piezoelectric antibacterial materials;

[0006] II. Achieving simple and efficient preparation;

[0007] Third, it can effectively ensure the practical application effect of powder-type piezoelectric antibacterial materials.

[0008] To achieve the above objectives, the present invention adopts the following technical solution.

[0009] A method for preparing an antibacterial piezoelectric material,

[0010] The preparation method includes:

[0011] According to the stoichiometry Ba 1-x Ca x Ti y Sn z Zr n O3 is taken from barium source, calcium source, titanium source, tin source and / or zirconium source, respectively, mixed evenly, and then added to ball milling media for initial ball milling to obtain pre-powder. After drying, the pre-powder is calcined at 1200-1280℃ for 3.5-4.5h, and then subjected to a second ball milling to obtain the antibacterial piezoelectric material.

[0012] Where: y+z+n=1, where 0<x<1, and 0<y<1, 0≤z<1, 0≤n<1.

[0013] Preferably, the initial ball milling is controlled at a ball milling speed of 300-500 rpm and a ball milling time of 12-36 h.

[0014] Preferably, the secondary ball milling control is set at a ball milling speed of 250–350 rpm and a ball milling time of 8–16 h.

[0015] An antibacterial piezoelectric material.

[0016] Application of an antibacterial piezoelectric material

[0017] The antibacterial piezoelectric material is used in the manufacture of bentonite-based antibacterial cat litter.

[0018] Preferably, the bentonite-based antibacterial cat litter is manufactured as follows:

[0019] Bentonite and the antibacterial piezoelectric material are mixed and ball-milled to obtain bentonite-based antibacterial cat litter.

[0020] Preferably, the bentonite is modified with tannic acid before being mixed with the antibacterial piezoelectric material.

[0021] Preferably, the modification treatment is as follows:

[0022] The modification process is completed by mixing bentonite and tannic acid, adding them to ball milling media, and then ball milling them.

[0023] Preferably, the mass ratio of bentonite to tannic acid is 1:(0.15-0.25).

[0024] In the technical solution of this invention, the most crucial step is to construct Ba. 1-x Ca xTi y Sn z Zr n O3, Ba 1- x Ca x Ti y Sn z Zr n O3 possesses excellent ferroelectric and piezoelectric properties. To achieve a high piezoelectric effect, the material needs to satisfy two conditions: high spontaneous polarization intensity and ease of perturbation of spontaneous polarization by an external field. These two conditions typically mutually restrict the piezoelectricity exhibited by the material. Furthermore, based on thermodynamic theory, it is clear that the piezoelectric constant is directly proportional to the product of spontaneous polarization intensity and dielectric constant. According to research by those skilled in the art, a larger dielectric constant indicates that spontaneous polarization is more easily perturbed by an electric field. Under mechanical force, barium titanate-based piezoelectric materials undergo deformation, which not only changes the polarization intensity of the crystal and enhances piezoelectricity but also generates electron-hole pairs, enhancing the separation and migration rate of charge carriers, thereby accelerating the generation of hydroxyl radicals and singlet oxygen. This achieves an antibacterial effect while promoting the migration of fibroblasts and macrophages. Characterization by the inventors revealed that the particles in the microstructure have distinct (001), (002), and (200) crystal planes, indicating that Ba… 1-x Ca x Ti 1-y X y O3 (X: Sn, Zr) has excellent piezoelectric properties.

[0025] However, during the construction of the aforementioned piezoelectric antibacterial materials, it is important to note that x should be controlled between 0.2 and 0.3, and y should be controlled between 0.5 and 0.6, to ensure that barium and titanium can constitute the main components.

[0026] Furthermore, through ball milling and composition control, the piezoelectric antibacterial material prepared by the present invention can ensure a high relative density [relative density = (actual density / theoretical maximum density) × 100%], ensuring that the piezoelectric antibacterial material of the present invention has a higher density, thereby ensuring that it has good mechanical properties.

[0027] In use, the piezoelectric antibacterial material of this invention can be effectively combined with common cat litter substrate bentonite. Before use, the bentonite needs to be treated with tannic acid. Tannic acid modification of bentonite allows the phenolic hydroxyl groups and benzene rings on the tannic acid to facilitate the dispersion of the piezoelectric antibacterial powder within the bentonite. The phenolic hydroxyl groups undergo esterification with the bentonite, thereby increasing the bonding strength. The synergistic effect of tannic acid modification and ball milling provides sufficient space for intercalation, enhancing the bonding strength between bentonite layers and improving the utilization rate of the bentonite. The layered stacking of bentonite significantly increases the specific surface area of ​​the material, resulting in better adsorption properties. Simultaneously, the introduction of numerous active groups such as hydroxyl and carboxyl groups increases the hydrophilicity of the bentonite, promoting the generation of active groups. Moreover, tannic acid has a polyphenolic hydroxyl structure, which can reversibly and dynamically combine with materials through hydrogen bonds, ionic bonds, coordination bonds and other means, making it easier for piezoelectric materials to be adsorbed on the (001) crystal facet. The highly exposed (001) polar crystal facet can not only directionally adsorb piezoelectric materials and have a large adsorption capacity, thus improving the piezoelectric catalytic activity of the material, but also provide more force sites, which can easily change the asymmetry of the piezoelectric material, thereby forming charges and improving the piezoelectric performance.

[0028] Through the above-mentioned directional adsorption, when the piezoelectric antibacterial material of the present invention is used to manufacture bentonite-based antibacterial cat litter, the bentonite can effectively apply external force to the (001) crystal plane of the piezoelectric antibacterial material after absorbing liquid and swelling, so as to ensure that it can generate effective polarization, so that the bentonite-based antibacterial cat litter has a positive charge on its surface after absorbing liquid and swelling, producing a significant antibacterial effect, and ensuring that effective antibacterial polarity is maintained.

[0029] In the process of combining piezoelectric antibacterial materials with bentonite, this invention uses ball milling to provide short-range in-situ energy, thereby promoting ion diffusion, increasing the layered structure of bentonite, expanding the interlayer of bentonite, and roughening the surface of bentonite. By ball milling, piezoelectric materials and modified bentonite are effectively fused together, achieving broad-spectrum antibacterial properties and high antibacterial rate of bentonite, while also preparing uniform piezoelectric antibacterial powder.

[0030] The bentonite prepared in this invention does not require the introduction of other antibacterial ions or organic antibacterial agents. Instead, it relies on the inorganic piezoelectric antibacterial material to generate an internal polarized electric field under external mechanical force (vibration, water flow, etc.), driving electron / hole migration and generating active groups on the surface. No external power source or special stimuli are required. This invention is of great significance for the development of highly efficient disinfection products and for broadening the application fields of bentonite. This invention prepares a bentonite with piezoelectric antibacterial properties by organically fusing piezoelectric antibacterial powder with tannic acid-modified bentonite. This bentonite exhibits a strong piezoelectric antibacterial effect and long-lasting stability, showing highly efficient and durable antibacterial effects against Escherichia coli and Staphylococcus aureus. The modified bentonite has high stability, a dense structure, and high mechanical strength. Ball milling yields a pulverized, well-dispersed material. Based on these materials, this invention provides a bentonite material with long-lasting antibacterial properties and a wide range of applications using piezoelectric antibacterial properties.

[0031] The beneficial effects of this invention are as follows:

[0032] 1) The preparation process of this invention is simple and the preparation cost is low;

[0033] 2) The materials prepared by this invention have good mechanical properties and good biocompatibility;

[0034] 3) The material prepared by the present invention can exhibit excellent long-lasting antibacterial properties under mechanical stimulation in the surrounding environment. Attached Figure Description

[0035] Figure 1 This is a scanning electron microscope image of a piezoelectric antibacterial material obtained in Example 1 of the present invention.

[0036] Figure 2 This is a comparative diagram of the antibacterial test results of a piezoelectric antibacterial material obtained in Example 1 of the present invention. Detailed Implementation

[0037] The present invention will be further described clearly and in detail below with reference to specific embodiments and the accompanying drawings. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.

[0038] Unless otherwise specified, all raw materials used in the embodiments of the present invention are commercially available or obtainable by those skilled in the art; unless otherwise specified, all methods used in the embodiments of the present invention are methods mastered by those skilled in the art.

[0039] Example 1

[0040] Preparation of piezoelectric antibacterial materials:

[0041] According to the stoichiometry Ba 1-x Ca x Ti y Sn z Zr n O3 (x=0.20, y=0.60, z=0.20, n=0.20) was prepared by mixing barium carbonate, calcium carbonate, barium oxide, tin oxide and zirconium oxide. After mixing evenly, anhydrous ethanol was added at a material-to-liquid ratio of 1:5 and the mixture was ball-milled for the first time (500 rpm / 12 h) to obtain a pre-powder. After drying, the pre-powder was calcined at 1250℃ for 4.0 h. Then, anhydrous ethanol was added at a material-to-liquid ratio of 1:5 and the mixture was ball-milled for the second time (300 rpm / 12 h) to obtain the piezoelectric antibacterial material.

[0042] The piezoelectric antibacterial material prepared in this invention was characterized by SEM, and the characterization results are as follows: Figure 1 As shown.

[0043] from Figure 1 The characterization results show that the piezoelectric antibacterial material prepared in this example has an irregular granular structure, exhibiting a large specific surface area and a microstructure similar to common piezoelectric materials. Density characterization of the prepared piezoelectric antibacterial material revealed a relative density of 96.2%, indicating highly dense characteristics and good mechanical properties.

[0044] In addition, the antibacterial properties of the piezoelectric antibacterial material prepared in this example were characterized by testing.

[0045] Take 100 μL of a concentration of 10 7 A CFU / mL Staphylococcus aureus suspension was evenly spread on an agar plate. The experimental groups received 0.5 mg / mL of the prepared piezoelectric antibacterial material, while the group without the piezoelectric antibacterial material served as a blank control. After incubating overnight at 37°C, the colony count was observed. Characterization results are as follows: Figure 2 As shown.

[0046] Figure 2 The left image shows the characterization results of the blank control, and the right image shows the characterization results after adding the piezoelectric antibacterial material. The characterization results show that the piezoelectric antibacterial material of the present invention also exhibits excellent antibacterial properties under no external force conditions, with a sterilization rate of >99%.

[0047] Example 2

[0048] Based on the preparation process of Example 1, piezoelectric antibacterial material samples were prepared according to the parameters x, y, z, and n in the table below, and their relative density and antibacterial properties were characterized in the same way as in Example 1. The results are shown in the table below.

[0049] x= y= z= n= relative density Sterilization rate 0.15 0.60 0.20 0.20 97.3% 98.3% 0.25 0.60 0.20 0.20 96.1% >99% 0.30 0.60 0.20 0.20 95.2% >99% 0.35 0.60 0.20 0.20 93.2% >99% 0.40 0.60 0.20 0.20 88.4% 98.6% 0.20 0.45 0.20 0.35 96.3% 95.6% 0.20 0.50 0.20 0.0.30 95.9% >99% 0.20 0.55 0.20 0.25 96.1% >99% 0.20 0.65 0.20 0.15 96.1% >99% 0.20 0.70 0.20 0.10 95.8% >99%

[0050] The results above show that barium-based materials have a relatively small impact on the antibacterial properties of the piezoelectric antibacterial material of the present invention, but a significant impact on the mechanical properties of the material. Therefore, in order to ensure that the piezoelectric antibacterial material of the present invention maintains superior mechanical properties, it is necessary to ensure that it has a relatively large content of barium-based materials. As expected, titanium-based raw materials mainly affect the antibacterial properties of the material, so it is also necessary to ensure that the piezoelectric antibacterial material obtained has a high titanium content.

[0051] Application Example 1

[0052] Preparation of bentonite-based antibacterial cat litter:

[0053] Bentonite and tannic acid were mixed at a mass ratio of 1:0.2 as raw materials, and deionized water was added at a material-to-liquid ratio of 1:5 as the ball milling medium. The mixture was ball milled at 300 rpm for 8 hours to obtain modified bentonite.

[0054] Modified bentonite and the piezoelectric antibacterial material prepared in Example 1 were mixed at a mass ratio of 1:0.05 as raw materials. Anhydrous ethylene glycol was added as the ball milling medium at a material-to-liquid ratio of 1:5. The mixture was ball milled at 300 rpm for 12 hours to obtain bentonite-based antibacterial cat litter.

[0055] Take 100 μL of a concentration of 10 7 A CFU / mL Staphylococcus aureus suspension was evenly spread on an agar plate. In the experimental group, bentonite-based antibacterial cat litter was added at a ratio of 0.5 mg / mL, while the experimental group without bentonite-based antibacterial cat litter served as a blank control. After incubating overnight at 37℃, the colony count was observed and the sterilization rate was calculated.

[0056] Sterilization rate = [1 - (number of colonies in the experimental group / number of colonies in the blank control group)] × 100%.

[0057] The sterilization rate in the above tests was approximately 93.6%.

[0058] Furthermore, the prepared bentonite-based antibacterial cat litter was added to excess deionized water to swell and agglomerate. The agglomerated material was then crushed in a mortar and pestle, and passed through a 200-mesh sieve to obtain absorbent cat litter powder. The absorbent cat litter powder was then subjected to the same sterilization performance test as described above. 100 μL of a 10... 7A CFU / mL Staphylococcus aureus suspension was evenly spread on an agar plate. The experimental group received 0.5 mg / mL of the prepared absorbent cat litter powder, while the experimental group without absorbent cat litter powder served as a blank control. After incubating overnight at 37°C, the colony count was observed, and the sterilization rate was calculated.

[0059] Sterilization rate = [1 - (number of colonies in the experimental group / number of colonies in the blank control group)] × 100%.

[0060] The sterilization rate in the above tests was >99%.

[0061] As can be seen from the above application tests, the bentonite-based antibacterial cat litter prepared by this invention exhibits excellent piezoelectric antibacterial properties. After the bentonite carrier absorbs water and expands, its actual antibacterial ability is greatly enhanced. It can be expected that when used as cat litter, it can maintain a certain level of conventional antibacterial properties, and after absorbing liquid and agglomerating and expanding, its antibacterial performance will reach a second peak, achieving strong antibacterial effect. The cat litter prepared has excellent performance.

[0062] Application Comparative Example 1

[0063] Preparation of bentonite-based antibacterial cat litter:

[0064] Bentonite was used as raw material, and deionized water was added at a ratio of 1:5 as ball milling medium. After ball milling at 300 rpm for 8 hours, fine bentonite powder was obtained.

[0065] Bentonite fine powder and the piezoelectric antibacterial material prepared in Example 1 were mixed at a mass ratio of 1:0.05 as raw materials. Anhydrous ethylene glycol was added as the ball milling medium at a material-to-liquid ratio of 1:5. The mixture was ball milled at 300 rpm for 12 hours to obtain bentonite-based antibacterial cat litter.

[0066] Take 100 μL of a concentration of 10 7 A CFU / mL Staphylococcus aureus suspension was evenly spread on an agar plate. In the experimental group, bentonite-based antibacterial cat litter was added at a ratio of 0.5 mg / mL, while the experimental group without bentonite-based antibacterial cat litter served as a blank control. After incubating overnight at 37℃, the colony count was observed and the sterilization rate was calculated.

[0067] Sterilization rate = [1 - (number of colonies in the experimental group / number of colonies in the blank control group)] × 100%.

[0068] The sterilization rate in the above tests was approximately 93.3%.

[0069] Furthermore, the prepared bentonite-based antibacterial cat litter was added to excess deionized water to swell and agglomerate. The agglomerated material was then crushed in a mortar and pestle, and passed through a 200-mesh sieve to obtain absorbent cat litter powder. The absorbent cat litter powder was then subjected to the same sterilization performance test as described above. 100 μL of a 10... 7 A CFU / mL Staphylococcus aureus suspension was evenly spread on an agar plate. The experimental group received 0.5 mg / mL of the prepared absorbent cat litter powder, while the experimental group without absorbent cat litter powder served as a blank control. After incubating overnight at 37°C, the colony count was observed, and the sterilization rate was calculated.

[0070] Sterilization rate = [1 - (number of colonies in the experimental group / number of colonies in the blank control group)] × 100%.

[0071] The sterilization rate in the above tests was approximately 91.6%.

[0072] As can be seen from the above application tests, the direct combination effect of bentonite and the antibacterial piezoelectric material prepared by the present invention is relatively limited. After direct mixing, it can maintain antibacterial and sterilization performance similar to that of Application Example 1 under non-swelling conditions. However, the sterilization performance after swelling is even lower than that under non-swelling conditions. This is mainly because under non-directional stress, the piezoelectric antibacterial material structure contained in the bentonite-based antibacterial cat litter may exhibit opposite polarity, which leads to the cancellation of its antibacterial performance and a weakening of its antibacterial and sterilization performance.

[0073] Application Comparative Example 2

[0074] Preparation of bentonite-based antibacterial cat litter:

[0075] Bentonite was used as raw material, and deionized water was added at a ratio of 1:5 as ball milling medium. After ball milling at 300 rpm for 8 hours, fine bentonite powder was obtained.

[0076] Bentonite fine powder and the piezoelectric antibacterial material prepared in Example 1 were mixed at a mass ratio of 1:0.05 as raw materials. Anhydrous ethylene glycol was added at a material-to-liquid ratio of 1:5, and the mixture was ultrasonically vibrated for 2 hours to obtain bentonite-based antibacterial cat litter.

[0077] Take 100 μL of a concentration of 10 7 A CFU / mL Staphylococcus aureus suspension was evenly spread on an agar plate. In the experimental group, bentonite-based antibacterial cat litter was added at a ratio of 0.5 mg / mL, while the experimental group without bentonite-based antibacterial cat litter served as a blank control. After incubating overnight at 37℃, the colony count was observed and the sterilization rate was calculated.

[0078] Sterilization rate = [1 - (number of colonies in the experimental group / number of colonies in the blank control group)] × 100%.

[0079] The sterilization rate in the above tests was approximately 94.2%.

[0080] Furthermore, the prepared bentonite-based antibacterial cat litter was added to excess deionized water to swell and agglomerate. The agglomerated material was then crushed in a mortar and pestle, and passed through a 200-mesh sieve to obtain absorbent cat litter powder. The absorbent cat litter powder was then subjected to the same sterilization performance test as described above. 100 μL of a 10... 7 A CFU / mL Staphylococcus aureus suspension was evenly spread on an agar plate. The experimental group received 0.5 mg / mL of the prepared absorbent cat litter powder, while the experimental group without absorbent cat litter powder served as a blank control. After incubating overnight at 37°C, the colony count was observed, and the sterilization rate was calculated.

[0081] Sterilization rate = [1 - (number of colonies in the experimental group / number of colonies in the blank control group)] × 100%.

[0082] The sterilization rate in the above tests was approximately 87.6%.

[0083] As can be seen from the above application tests, the direct bonding effect between bentonite and the antibacterial piezoelectric material prepared by the present invention is relatively limited. After direct mixing, it can maintain antibacterial and sterilization performance similar to that of Application Example 1 under non-swelling conditions. However, the sterilization performance after swelling is even lower than that under non-swelling conditions. This is mainly because although ultrasonic vibration can also achieve effective directional bonding between modified bentonite and piezoelectric antibacterial material, the piezoelectric antibacterial material is attached to the outer surface of modified bentonite rather than inside the pores. After the bentonite swells, it does not exert a squeezing effect on its (001) crystal plane, but instead exerts a tension effect, causing a significant reversal of its surface polarity. This significantly weakens the actual swelling antibacterial and sterilization performance of the prepared bentonite-based antibacterial cat litter.

[0084] It is evident that the piezoelectric antibacterial material of the present invention has good antibacterial properties and exhibits unique piezoelectric antibacterial capabilities. However, the activation of this capability requires combining it with bentonite material with high water absorption and swelling rate in an appropriate manner; otherwise, it may weaken the antibacterial and sterilization performance of the piezoelectric antibacterial material itself.

Claims

1. An application of an antibacterial piezoelectric material, characterized in that, The antibacterial piezoelectric material is used in the manufacture of bentonite-based antibacterial cat litter; The antibacterial piezoelectric material was prepared using the following method: According to the stoichiometry Ba 1-x Ca x Ti y Sn z Zr n O3 was taken from barium, calcium, titanium, tin and zirconium sources, respectively, mixed evenly, and then added to ball milling media for initial ball milling to obtain pre-powder. After drying, the pre-powder was calcined at 1200-1280 °C for 3.5-4.5 h, and then subjected to a second ball milling to obtain the antibacterial piezoelectric material. Where: y+z+n=1, where 0<x<1, and 0<y<1, 0<z<1, 0<n<1; The bentonite-based antibacterial cat litter is manufactured by mixing bentonite with the antibacterial piezoelectric material and then ball milling the mixture to obtain the bentonite-based antibacterial cat litter. Before the bentonite is mixed with the antibacterial piezoelectric material, the bentonite is modified with tannic acid. The modification process is as follows: the bentonite and tannic acid are mixed and then ball-milled with ball milling media to complete the modification process. The mass ratio of bentonite to tannic acid is 1:(0.15~0.25).

2. The application according to claim 1, characterized in that, The initial ball milling control is set at a ball milling speed of 300–500 rpm and a ball milling time of 12–36 h.

3. The application according to claim 1, characterized in that, The secondary ball milling is controlled at a ball milling speed of 250–350 rpm and a ball milling time of 8–16 h.

Citation Information

Patent Citations

  • Preparation method of tetragonal-phase barium titanate ceramic powder with antibacterial property

    CN113716954A

  • Pet cat litter easy to absorb water and deodorize and preparation method thereof

    CN115968793A

  • Lead-free piezoelectric ceramic material with low resistance and high power generation performance and preparation method thereof

    CN116655375A